Clarification on WPS Applicability for SS316L to Duplex Welding per ASME Section IX

108 views
Skip to first unread message

Nambirajan Avudaiappan

unread,
May 1, 2025, 4:11:08 AM5/1/25
to material...@googlegroups.com

Dear Experts,

I hope this message finds you well.

I would like to seek your clarification regarding the applicability of an existing WPS.

We have successfully qualified a WPS for welding SS316L to Super Duplex using ER2594 filler metal. Both base materials are classified under P-No. 8 to 10H, and the filler metal falls under F-No. 6.

However, our actual production requirement involves welding SS316L to Duplex Stainless Steel using ER2209, which also falls under F-No. 6, and the base metals remain under P-No. 8 to 10H.

As per ASME Section IX, since the base metal P-Numbers and filler metal F-Numbers remain unchanged, could you please confirm whether the existing WPS is valid for this application as well, or if a new qualification is required?

Thank you in advance for your guidance and support.

Regards,

Nambirajan A

Ranjit singh

unread,
May 1, 2025, 7:04:07 AM5/1/25
to material...@googlegroups.com
Dear sir,

We are facing problem in welding crack for desimilar metal like en19 hub dia 350mm thick 200mm and shaft en19 dia 140mm groove weld 28mm.

Process:- SMAW
Pre heating 200-250 degree.
Observation:- crack 

Regards,

Ranjit
9216671043

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJuyB2XnCz1x1PWFoGvwdFQQCG-e_8K_ksgtNPtt2mwocbS4Gw%40mail.gmail.com.

Nambirajan Avudaiappan

unread,
May 1, 2025, 9:28:00 AM5/1/25
to material...@googlegroups.com
Dear ranijith,
My question regarding the applicability of WPS only.

Deerendra Karanth

unread,
May 1, 2025, 2:03:03 PM5/1/25
to material...@googlegroups.com

If supplementary requirements for impact testing are applicable, a change in A-number will require new WPS qualification; however, if impact testing is not required, the existing WPS can be used as long as the P-Number and F-Number remain unchanged.

BR, 

Deerendra.. 



Vishwas Keskar

unread,
May 1, 2025, 10:30:41 PM5/1/25
to material...@googlegroups.com, material...@googlegroups.com
P10 H to P8 
ASME sec IX 
WPS is acceptable
If API582 or other Client specifications are applicable , then revisit the decision.
Review Discuss with QA ,Welding proceed accordingly 
Sent from my iPhone

On 1 May 2025, at 11:32 PM, Deerendra Karanth <dkar...@gmail.com> wrote:



Nambirajan Avudaiappan

unread,
May 1, 2025, 11:48:10 PM5/1/25
to material...@googlegroups.com
Thanks Vishwas sir, let me check with Customer specification once again. 

Best Regards, 
Nambirajan A