Dear Welding Experts,


We have recently completed PQR qualification on a 220 mm thick joint using a combination of SMAW + SAW processes. 

Material-SA 5160 GR.70 

  • SMAW deposited thickness: 111 mm(E7018-1)

  • SAW deposited thickness: 109 mm(EH10K)


I now need to prepare a WPS for the SMAW process only. Could you please clarify up to what thickness this WPS will be qualified for based on the deposited SMAW thickness?

Best Regards

Pankaj

Saurabh Jain

unread,
Aug 12, 2025, 9:33:13 AMAug 12
to material...@googlegroups.com
As per sec IX

Without impact 5mm to 1.33T, 
With impact 16mm to 1.33T

Max deposit thickness also 1.33T


Regards 
Saurabh Jain

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAJF_nWOGv24pUQHerd_WTUQJXcrCJSoteFRGkdZwMzwGrgidXQ%40mail.gmail.com.

pankaj pachahara

unread,
Aug 12, 2025, 9:57:34 AMAug 12
to material...@googlegroups.com
So our max deposit thickness in WPS will be -220X1.33 =292.6

We will not consider the thickness we have deposited by smaw process.

We will consider Our PQR test coupon 220 thick. 
 

sridhar cn

unread,
Aug 12, 2025, 12:24:33 PMAug 12
to material...@googlegroups.com
One out of way query:
Why use SMAW process for a 111 mm thick weld deposit? SAW is OK for balance 109 mm thickness.
SMAW is inefficient compared to GMAW/FCAW  processes. They have an efficiency of 85 to 90%  
compared to 30-40% in SMAW (due to use of E 7018) and will reduce your welding time and cost factor.
Think for a better change!
C Sridhar.

--

pankaj pachahara

unread,
Aug 12, 2025, 1:15:56 PMAug 12
to material...@googlegroups.com
We have made SMAW+SAW WPS but now using that previous PQR we will qualify SMAW process for nozzle in Boilers we don’t have approved WPS for GMAW/FCAW so that’s why we need to make for SMAW. 

Best Regards
Pankaj 

sridhar cn

unread,
Aug 13, 2025, 6:00:55 AMAug 13
to material...@googlegroups.com
Understood, and thanks for the clarification. For a nozzle joint welding in a boiler, third party
agencies allow SMAW process in general.