Alloy 20 material Uns no8020. Which filler wire suitable?? Can I use ER320 Filler wire.

sivakumar kaliyamoorthy

未讀,
2020年10月24日 上午8:58:222020/10/24
收件者:material...@googlegroups.com
Hi,

In most Ni alloys ( ASME II B-N625,825,8020 ) filler wire is used ER NiCrMo-3 , Ni-58,Cr-23,Mo-10 maximum.
ER 320 has chemistry Ni-36 , Cr-21, Mo-3 max only, so it cannot be used for Ni alloys.

Thanks and Regards,

Sivakumar. K

On Fri, Oct 23, 2020 at 8:03 AM Solai Murugan <sola...@gmail.com> wrote:
Dear sir.
Alloy 20 material Uns no8020. Which filler wire suitable?? Can I use ER320 Filler wire.

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHPVRABrExyjtT6XWp5Z7vR61VrfxbB7X%2Bg%3DWac-XOiScECVdQ%40mail.gmail.com.

Vishwas Keskar

未讀,
2020年10月26日 凌晨12:42:002020/10/26
收件者:material...@googlegroups.com
Yes 
you can use 

use ER320LR 



Regards

On Fri, Oct 23, 2020 at 8:03 AM Solai Murugan <sola...@gmail.com> wrote:
Dear sir.
Alloy 20 material Uns no8020. Which filler wire suitable?? Can I use ER320 Filler wire.

回覆所有人
回覆作者
轉寄
0 則新訊息