SA-516 Gr 70

116 views
Skip to first unread message

Kishore S

unread,
Jul 15, 2022, 2:23:24 AM7/15/22
to Materials & Welding
Dear sir 

what are the step to find an electrode for SA516 gr 70 in the internet they have mentioned E7018 but as per the SAIL TEST CERTIFICATE tensile strength is 79ksi so what electrode do I have to use   

Rameshbabu B

unread,
Jul 15, 2022, 3:31:16 AM7/15/22
to material...@googlegroups.com
E 7018 is the correct one. The sail test certificate mentions the observed values nothing to worry about it. 


On Fri, Jul 15, 2022 at 12:31 PM Kishore S <kishor...@gmail.com> wrote:
Dear sir 

what are the step to find an electrode for SA516 gr 70 in the internet they have mentioned E7018 but as per the SAIL TEST CERTIFICATE tensile strength is 79ksi so what electrode do I have to use   

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/ab5513fa-c564-40ce-953a-f67e68a3ea03n%40googlegroups.com.


--

Ramesh Babu Balaram

Corporate Head, Quality

The Oriental Towers, No. 461, 1st Floor, 17th Cross Road, 4th Sector,

Sector 4, HSR Layout, Bengaluru, Karnataka 560102.

M 9840531355  E ramesh...@zetwerk.com  W zetwerk.com

App Green Footer Image Please consider your environmental responsibility. Before printing this e-mail message, ask yourself whether you really need a hard copy.



This information may be confidential and/or privileged. Use of this information by anyone other than the intended recipient is prohibited. If you receive this in error, please inform the sender and remove any record of this message

james gerald

unread,
Jul 15, 2022, 3:31:17 AM7/15/22
to material...@googlegroups.com
What is your application and what is the design and fabrication code


--

Mohammed Abdulsayeed76

unread,
Jul 15, 2022, 3:31:17 AM7/15/22
to Materials-Welding
Dear Kishore,
Based on the tensile strength 79 KSI. You can use  low hydrogen electrode E8018
Regards 
Sayeed



On Jul 15, 2022 at 11:53 AM, <Kishore S> wrote:

Dear sir 

what are the step to find an electrode for SA516 gr 70 in the internet they have mentioned E7018 but as per the SAIL TEST CERTIFICATE tensile strength is 79ksi so what electrode do I have to use   

--

Anilkumar G

unread,
Jul 15, 2022, 3:41:15 AM7/15/22
to material...@googlegroups.com
E7018. If you have plan to do normalizing after welding go for E8018

Regards
Anilkumar

On Fri, Jul 15, 2022 at 11:53 AM Kishore S <kishor...@gmail.com> wrote:
Dear sir 

what are the step to find an electrode for SA516 gr 70 in the internet they have mentioned E7018 but as per the SAIL TEST CERTIFICATE tensile strength is 79ksi so what electrode do I have to use   

--

Vishwas Keskar

unread,
Jul 15, 2022, 4:49:26 AM7/15/22
to material...@googlegroups.com
SA 516 Gr 70 Means 70KSI  or 490 MPa is minimum UTS required was per SA 516. for these plates.

Compatible electrode  is E7018  as 
minimum UTS of this electrode is 70KSI minimum or 490MPa minimum. 

This is Welding and Material Technology compatibility and acceptable to Code requirements. 


On Fri, 15 Jul 2022, 11:53 Kishore S, <kishor...@gmail.com> wrote:
Dear sir 

what are the step to find an electrode for SA516 gr 70 in the internet they have mentioned E7018 but as per the SAIL TEST CERTIFICATE tensile strength is 79ksi so what electrode do I have to use   

--

Kannayeram Gnanapandithan

unread,
Jul 16, 2022, 9:04:39 AM7/16/22
to materials-welding
u have to match minimum tensile strength. in ur case, 516 gr 70 means minimum tensile is 70000psi or 485 Mpa. To match this, u can very well use 7018 which is 70000 psi or 485 Mpa. U are not supposed to match with actual tested value because it will vary. 

On Fri, Jul 15, 2022, 11:53 AM Kishore S <kishor...@gmail.com> wrote:
Dear sir 

what are the step to find an electrode for SA516 gr 70 in the internet they have mentioned E7018 but as per the SAIL TEST CERTIFICATE tensile strength is 79ksi so what electrode do I have to use   

--

Venkatachari Muralidharan

unread,
Jul 17, 2022, 12:50:18 AM7/17/22
to material...@googlegroups.com
Go for E 8018 electrode 

Sent from my iPhone

On 16-Jul-2022, at 6:34 PM, Kannayeram Gnanapandithan <kgpan...@gmail.com> wrote:



srinivas rao

unread,
Jul 17, 2022, 11:21:34 PM7/17/22
to Materials & Welding

Dear Kishore , 
consuamble selction is mainly depends on  Base metal  tensile properties , Specification and service requirements(Hardness and impact requiremnts). other facrtor also to be taken into considered in case if you wan to fo with different welding processes ,in your  case it is already SMAW process  and  base metrial is  SA 516 Gr 70 means minimum specified tensile strength is 70000psi /485 Mpa. while selecting consumable you need to consider the minimum specified stregth of the base metal not acutal tensilet stregth  specified in MTC , so the recommended  electode for this purpose is E7018 which satisfys the base mental strength requirement for impact requirements to be confirmed by manufaturer based on your project requiremnts, over matching consuambes are not required in this regard as many of the applications E7018/E7018-1 will suffice the requirement of cleints .

in some applications if your project impact reuirements are at below -46deg C you may need to choose E8018/E8018-C3 elctrodes.


Thanks & Regards,
Srinivas Rao 
welding Engineer

Kannayeram Gnanapandithan

unread,
Jul 18, 2022, 2:25:14 AM7/18/22
to materials-welding
In addition , pl check whether it is subjected to PWHT, if so, basically 15mps will be lost due to SR, in that select 7018-1
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349