Please reply with your valuable comments, details are as follows.

Welding Process : FCAW
Material : SA 516 Gr.70 N, 20 mm Thickness
PWHT : 610 ° C ± 10° C, @ 120 Minutes
Tensile, Bend, Macro & Hardness Values are Accepted.
But in the Charpy Impact Test @ -28° C  , Average on WCL is 09 Joule
In HAZ the average is 217 Joule.

Filler Wire Details
K-71T1-C1, AWS A5.20, 1.2 mm Diameter
Impact Values (as per MTC) , Charpy V-Notch -20° C, Avg. 54 J & Min. 27 J

Thank You & Regards
Williams P Wilson
QA/QC Engineer
Please consider the environment before printing this message

williams p wilson

unread,
Sep 22, 2022, 3:33:15 AM9/22/22
to material...@googlegroups.com
Dear Experts,
Greetings!!

Anyone knows the reason for very low impact test values on the weld centerline.
Thanks in advance.

Pravin Kurade

unread,
Sep 22, 2022, 4:37:14 AM9/22/22
to material...@googlegroups.com
Hello which consumables you used to weld this joint

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAHBxnQ4SU5G3mR6obs_Lhus0_%2BHvE5NJoAhv21N_NREYHqmFww%40mail.gmail.com.
--
Pravinkumar kurade

williams p wilson

unread,
Sep 22, 2022, 4:44:08 AM9/22/22
to material...@googlegroups.com
FYI

Kiswel Brand Flux Cored Wire - E71T1-C1


Thank You & Regards
Williams P Wilson
QA/QC Engineer
Please consider the environment before printing this message

Ahmed Osman

unread,
Sep 25, 2022, 2:50:37 AM9/25/22
to material...@googlegroups.com
- try to use mixed gas ( argon , CO2 ) instead of pure co2
- reduce as much the layers thickness 
what was the max. hardness value for in the root pass  and in the cap ?   

Best Regards ,
ENG. Ahmed Osman



williams p wilson

unread,
Sep 25, 2022, 11:24:27 PM9/25/22
to material...@googlegroups.com
Dear Sir,
FYI

what was the max. hardness value for in the root pass  and in the cap ?   
Root Pass : 224 HV10 & Capp : 198 HV10 