Dear sir / experts,
I need help for welding a M.S. Pipe with Mechanized FCAW Process for root pass to get good penetration for X-ray ( without backing strip & back gouging ) Wire, E71T-1. Dia, 1.2 mm. Shielding Gas, 100 % CO2. Pipe Dia 200mm. Wall Thickness 08.00mm. Welding Position 1GR.
Please give me some guidelines for above welding operation . Like, voltage, Amps, and wire speed, travel speed, stick out, torch angle, gas flow rate for root run & other subsequent run.
Few Engineers say that FCAW are not be recommended for open root run. They advised for root run weld with GMAW process & subsequent run by FCAW process. And I found in ESAB Welder Guide Book . Page No. 16. they are also not recommended root run by FCAW. on Pipe & Plate both.
My queries are as follows :
1. Is it possible to weld a root run for X quality penetration with FCAW Process?
2. There is any restriction for root run welding with FCAW by any Welding Codes like ASME Sec. IX, AWS D1.1. or ISO 15614. ?
Thanks & Regards.
G. K. Banerjee.
Welder Trainer.
NAGPUR. ( India )
M-09764555112. 09423632112.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b4e51fdb-f051-4436-9470-46f5cc943446%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
FCAW not recommended as it is high heat input process . The toughness of the root is affected . The most important is to control the heat input at root as it is the most important run in the weld . That why GTAW is mostly recommended and it's a clean process . STT Lincoln or RMD miller is ideal as the current characteristic is well controlled and therefore the heat input . So to be on safer avoid FCAW for X-ray quality weld .
1. It will be difficult to get consistent root penetration for 8.00 mm thick 200 mm dai.pipe using 1.20 mm wire in FCAW manual or auto process. It may work out for a higher thicknessand larger size.2. For 8 mm thick. 0.80 could be ideal and that size is not available in FCAW process.3. Using GMAW (+) FCAW is gain not practical for 8 mm thick and also not economical.4. GMAW process with Argon + CO2 as shielding gas may help with two pass technique.Again, LF may at times may affect X-ray quality5. Alternatively you can try Pulsed Auto TIG process with Argon gas. It may meet your requirement.Sridhar.09444971077
Sent: Wednesday, 5 October 2016 9:53 PM
Subject: [MW:25487] Re: Open Root Pipe Welding / Groove Welding with FCAW Process
STT process - LINCOLN will give excellent root pass quality including RT satisafctory--
On Tuesday, October 4, 2016 at 2:06:35 PM UTC+5:30, Gopi Krishna Banerjee wrote:Dear sir / experts,I need help for welding a M.S. Pipe with Mechanized FCAW Process for root pass to get good penetration for X-ray ( without backing strip & back gouging ) Wire, E71T-1. Dia, 1.2 mm. Shielding Gas, 100 % CO2. Pipe Dia 200mm. Wall Thickness 08.00mm. Welding Position 1GR.Please give me some guidelines for above welding operation . Like, voltage, Amps, and wire speed, travel speed, stick out, torch angle, gas flow rate for root run & other subsequent run.Few Engineers say that FCAW are not be recommended for open root run. They advised for root run weld with GMAW process & subsequent run by FCAW process. And I found in ESAB Welder Guide Book . Page No. 16. they are also not recommended root run by FCAW. on Pipe & Plate both.My queries are as follows :1. Is it possible to weld a root run for X quality penetration with FCAW Process?2. There is any restriction for root run welding with FCAW by any Welding Codes like ASME Sec. IX, AWS D1.1. or ISO 15614. ?Thanks & Regards.G. K. Banerjee.Welder Trainer.NAGPUR. ( India )M-09764555112. 09423632112.
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b4e51fdb-f051-4436-9470-46f5cc943446%40googlegroups.com.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/1561857038.504976.1477817507432%40mail.yahoo.com.