Method of Heat treatment - HT using Electric Resistance Pads suitable to achieve temperature of 1000 Deg C
Loading at or below - 200 Deg C
Rate of Heating - 200 Deg C / hr
Holding temperature - 920 +/- 10
Deg C
Holding time - 125 minutes
Rate of Cooling - Remov Electric Resistance Pads
after holding period is over - Forced Air cooling - Use Dry Air Blast
Unloading at or below - Room temperature
Note - The job shall be supported suitably to avoid distortion of PIping spools .
attach thermocouple as per Pipe diameter .