ER 70S-2 in pipeline root welding as per API 1104

169 views
Skip to first unread message

K.M Hrishikesan

unread,
May 2, 2024, 5:44:59 AM5/2/24
to materials-welding
Hi

One of our contractors wants to qualify a PQR using root with ER 70S-2 and subsequently with E 8010-1. I have never come across root being welded with GTAW in pipeline. Can any one comment please..??

Regards
Hrishikesan 

ARORA Rajeev

unread,
May 2, 2024, 6:12:45 AM5/2/24
to materials-welding
Can be .. we are using in sour services pipeline to reduce root repair 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFHBd_-V4-xRqYnV9k2fbaBoeqgyhyLRE9E9yRv3mS9WkE952Q%40mail.gmail.com.

Lakshman

unread,
May 2, 2024, 6:12:52 AM5/2/24
to material...@googlegroups.com

Hi
What is the base material, size and groove ?

 

Technically Nothing wrong in using GTAW with ER70S-2.

Pls do proper PQR, in one of the project I used GTAW for root

All the best

 

Thanks & Regards,

Lakshman Kumar.

+91 9440031459

--

K.M Hrishikesan

unread,
May 2, 2024, 6:21:30 AM5/2/24
to materials-welding
Thanks Mr Lakshman...Base material is API 5L X70. Thickness 24 mm, single V groove. Could you please  share the WPS of the project you mentioned?

Thanks..

ARORA Rajeev

unread,
May 2, 2024, 11:39:55 AM5/2/24
to materials-welding
This pipeline is sour or nonsour service?

K.M Hrishikesan

unread,
May 2, 2024, 11:39:55 AM5/2/24
to materials-welding
Thanks Mr Rajiv.. Could you please  share the WPS relevant pages?

Kannayeram Gnanapandithan

unread,
May 2, 2024, 11:57:21 AM5/2/24
to materials-welding
ER 70S3 is the best for pipeline 

K.M Hrishikesan

unread,
May 2, 2024, 11:57:21 AM5/2/24
to materials-welding

Amol Betkar

unread,
May 3, 2024, 4:28:09 AM5/3/24
to material...@googlegroups.com

Dear,

In accordance with API 1104, the standard for welding of pipelines and related facilities, the root pass welding for pipelines is typically performed using Shielded Metal Arc Welding (SMAW), also known as manual metal arc welding or stick welding. Gas Tungsten Arc Welding (GTAW), commonly referred to as Tungsten Inert Gas (TIG) welding, is not typically recommended for root passes in pipeline welding according to API 1104.

While API 1104 doesn't explicitly prohibit the use of GTAW for root pass welding, it emphasizes SMAW as the primary method for root pass welding due to its suitability for pipeline welding applications. ER 70S-2 filler material is more commonly associated with Gas Metal Arc Welding (GMAW) or MIG welding, rather than SMAW or GTAW, and may not provide the desired properties for root pass welding in pipeline applications.

For subsequent passes after the root, API 1104 often recommends the use of specific filler materials such as E 8010-1, which is designed for pipeline welding applications. This electrode is commonly used for root and hot pass welding in pipeline construction due to its ability to provide deep penetration and excellent mechanical properties.

In summary, while GTAW may not be explicitly prohibited by API 1104, SMAW using appropriate filler materials such as E 8010-1 is generally the preferred method for root pass welding in pipeline construction, ensuring compliance with industry standards and specifications.

Regards,

Amol K.Betkar


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAFHBd_-V4-xRqYnV9k2fbaBoeqgyhyLRE9E9yRv3mS9WkE952Q%40mail.gmail.com.


--
Best regards,

Amol K.B
B.E(Mech), CSWIP 3.2.2, NACE CIP 1 & ASNT LII(4M)

K.M Hrishikesan

unread,
May 3, 2024, 8:25:19 AM5/3/24
to material...@googlegroups.com
Dear Mr Amol

Could you please quote the specific reference from API 1104 that prohibits GTAW for root welding?

Muhammad Asif

unread,
May 3, 2024, 11:59:20 AM5/3/24
to material...@googlegroups.com
Dear Mr. Amol, 
Can you please share the specific clause which states that we can not use GTAW in pipelines?

Amol Betkar

unread,
May 4, 2024, 1:50:55 AM5/4/24
to material...@googlegroups.com

Dear,

API 1104, "Welding of Pipelines and Related Facilities," does not specifically prohibit Gas Tungsten Arc Welding (GTAW) for root welding. The choice of welding process for root pass welding is typically governed by the specific project requirements, welding procedure specifications (WPS), and applicable industry standards and codes.

However, API 1104 does provide guidelines and requirements for the welding process, including the root pass, such as ensuring proper penetration, fusion, and alignment. It also outlines acceptance criteria for welds, including visual inspection and non-destructive testing (NDT) methods. So, while it doesn't specifically prohibit GTAW, it sets standards for the quality and integrity of welds regardless of the welding process used.



Vinay

unread,
May 5, 2024, 7:47:15 AM5/5/24
to material...@googlegroups.com
We Have done    GTAW with ER70S-2