What are equivalent consumables for ER310 ? ER310 to 316L ?

52 views
Skip to first unread message

PK M

unread,
Sep 23, 2025, 6:06:49 AMSep 23
to material...@googlegroups.com

Dear All,

Gas Tip material SS310.

Company Specification says use 316L filler Wire, can we use filler wire SS316L?

What are equivalent consumables for ER310  ?   ER310 to 316L ?

Please give your suggestions. Explain with reference.


Thanks,

PKM

venkateswara reddy Desireddy

unread,
Sep 23, 2025, 6:44:39 AMSep 23
to material...@googlegroups.com
For ss310, ER 310 is good. ER 316L also we can use.


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAFoQ_nd-bF%3Dbj%2B_GofZGy-Y5LmuqmY4WBDT-Cc7O3eDBJBOhpA%40mail.gmail.com.

sridhar cn

unread,
Sep 26, 2025, 5:49:44 AMSep 26
to material...@googlegroups.com

 

 Type 310 has 24-26% Cr and 19-22% Ni, and is suitable for High temperature service up to ~1100-12600C. 

 Mostly used for furnace parts (cement industries), heat treatment baskets, burners, etc.  

 Type 316 has 16-18% Cr,11-14% Ni, and 2-3% Mo and is suitable for service temperature up to ~800-860 °C,                                 i.e., weaker at high Temperatures. Hence, not recommended (due to differences in composition and resulting                        mechanical properties) for welding 310 due to the risk of hot cracking, loss of oxidation resistance. So, the use                                     of 316L is incorrect unless the design service is very mild (not a high temp.) and the client accepts the responsibility.

 The matching consumable for 310 is E/ER310. In case you want to join 310 to 316L (dissimilar joining), use                                       E/ER 309MoL or ERNiCr-3 (Inconel 82) for critical or cyclic service.

 

 C Sridhar.


--