55 views
Skip to first unread message

Shaik Meraj

unread,
Jun 15, 2023, 5:51:28 AM6/15/23
to Materials & Welding
Dear Experts

We have prepared SS PQR with 316 PIPE and ER316L filler

Right now we have project of SS304 to SS304 1 1/2"pipe welding for flocculant service.

As changing filler classification from PQR to WPS is supplementary variable as per ASME SEC IX.
 
Can I use my SS PQR 316 to prepare wps for ss304 to ss304 by changing only filler material to er308 (in pqr it is er316L) as both material falls in same P no and group no.

Can I strongly justify my point of changing filler classification er316L to er 308 in wps without undergoing any additional testing or procedures.

Kindly suggest the strong points with standards if any.

Thank you in advance 

Raghuram Bathula

unread,
Jun 15, 2023, 5:56:42 AM6/15/23
to material...@googlegroups.com
yes you can revise WPS as A, P numbers will be same 

--

Pham Thanh Tinh

unread,
Jun 15, 2023, 5:59:07 AM6/15/23
to material...@googlegroups.com
Please check design temperature and fluid service, if impact test requirement you can not do. if impac test requirement you can do that. 

Vào Th 5, 15 thg 6, 2023 vào lúc 12:51 Shaik Meraj <123sha...@gmail.com> đã viết:
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/179b6dd3-2ea8-4fe8-b718-8890c6d9d1e4n%40googlegroups.com.


--
Best & Regard
Pham Thanh Tinh
QC Manager
China National Chemical Engineering Third Co.LTD
South Ghawar Gas Separation Plant & Associated Facilities Project
Mobile phone +966. 556802308 


Kannayeram Gnanapandithan

unread,
Jun 16, 2023, 1:28:04 AM6/16/23
to material...@googlegroups.com
u can, but generally when u prepare WPS, u can mention like 308 for 304, 316 for 316 etc in single wps except where Ano changes
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


--

Shaik Meraj

unread,
Jun 16, 2023, 12:58:26 PM6/16/23
to Materials & Welding
Thanks for the quick response.

The operating pressure is 800 kpag at 30 degrees C
The Designed pressure is 1000Kpag at 100degrees C

Kindly clarify will any sort of test is applicable to prepare WPS now. (I don't want to go in any extra procedures)