Nitrid Precipitation in Duplex SS (ISO 17781 QLll)

24 views
Skip to first unread message

Ilkin Hasanov

unread,
Mar 17, 2021, 11:07:46 PM3/17/21
to material...@googlegroups.com
Hi All,

Could you please advise,
If during micro-structural analyse  it were observed Nitrid Precipitates , how need to evaluate test results (mechanical test was done according ISO17781 QL 2)
I want to note that, Specimens were taken for WPQT of Duplex SS, MDT is -25Celsius
PQT coupon dimensions are WT=18mm OD=168.3mm.
Corrosion test results are acceptable ,There was no observed any pittings & Charpy V test results are acceptable (@-46celsius)


Regards, 
Ilkin Hasanov.

Ahmed Osman

unread,
Mar 18, 2021, 1:28:42 AM3/18/21
to material...@googlegroups.com
Dear Ilkin Hasanov ,

 Acceptance of Nitrid precipitations is depending on if CVN and ASTM G 48 test passed or not .. just to be recorded in the report  


Best Regards ,
Ahmed Osman



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADrxeDam%2BqjauoyQHuY274tVCom4GRzoWEr0umXVKN7ScuwO-A%40mail.gmail.com.
Reply all
Reply to author
Forward
0 new messages