AWS A 5.9 ER410 is the filler wire.
Considering the carbon and Chromium content, looking for a preheat of 200°C with maximum interpass as 315°C.
I take it ,No interruption during welding will be good for joint. Material will be constantly maintained at the minimum preheat temperature during welding.
For post weld heat treatment , I am thinking of bringing the material to 100°C (This is to ensure that there is complete transformation of the weld and HAZ to martensite ) and then follow this with PWHT for 4 hours.
I am thinking of tempering temp of 610°C ( 20°C below tempering temperature of the material).
Any recommendation in this regard will be greatly appreciated.
Thanks & best regards
Vikas
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACpSjO%3Dnw0gymJLohpEzJ3aWuz7y462ASyMioCY3KnMWXHb7Fw%40mail.gmail.com.
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CACpSjO%3Dnw0gymJLohpEzJ3aWuz7y462ASyMioCY3KnMWXHb7Fw%40mail.gmail.com.