SS 405 grains

64 views
Skip to first unread message

EmaD FaRaHanI

unread,
Jan 24, 2021, 10:42:58 PM1/24/21
to material...@googlegroups.com
Dear all,

what will happen to the grains of a ferritic stainless-steel type AISI 405 used as an attachment of a hanger bar in a boiler, when it is exposed to flame temperatures of the boiler for 4 years of continuous operation? It is understood that the 405 steel will not oxidize in the high-temperature service environment.

Regards,

Emad


Ahmed Osman

unread,
Jan 25, 2021, 12:46:13 AM1/25/21
to material...@googlegroups.com
may get :-
 *  grain growth which lead to low toughness 
 *  brittle phases as Sigma or Chi which lead to loos of toughness or even cracking 

Best Regards ,
ENG. Ahmed Osman


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CABtwbJG4D61j93y-Onv4L1kOjgxaAhSTDaCUgJ_9MjhzSm_4nA%40mail.gmail.com.

Vishwas Keskar

unread,
Jan 26, 2021, 1:45:12 AM1/26/21
to material...@googlegroups.com
Is welding involved ?
If yes , what welding procedure ?
Pl. let us know 

What thickness are involved ?

Vishwas Keskar Welding Manager WELDING

unread,
Jan 31, 2021, 10:13:52 PM1/31/21
to Materials & Welding
These are straight Cr Stainless steels for high temperature application.
In boiler , you can use this material.
Pl. send what attachment part you are looking for ?

EmaD FaRaHanI

unread,
Jan 31, 2021, 10:31:13 PM1/31/21
to material...@googlegroups.com
Thank you for your answer. I was wondering what would happen to grains of stainless steel 405 grains as hanger in boiler  when they exposed to high temperature for long time?

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.

pgos...@rogers.com

unread,
Jan 31, 2021, 10:54:20 PM1/31/21
to material...@googlegroups.com

Hi Emad,

 

Your query does not provide details about design/working condition.405 is a ferritic stainless steel. These steels have “good oxidation resistance “however lacks the ductility which is  well evident in austenitic stainless steel. 475 Deg embrittlement may be a possibility upon prolonged exposure @ 500 Deg or more. Read the attached extract from API-RP-571 and proceed for any inspection/ damage assessment as required.

 

Hope this would be of help.

Thanks.

 

Pradip Goswami.P.Eng, IWE.

Independent  & Consulting Welding & Metallurgical Specialist

Linkedin: https://www.linkedin.com/in/pradip-goswami-2999855/

Email:pgos...@rogers.com,pradip....@gmail.com

Cell/Whasapp:1-905-9793232

Section_4 General Damage Mechanisms_475Deg C Embrittlement.pdf