Dear Group Members,

We are working with material SA 335 P9 8mm thickness, which has a P number of 5B. For welding this material, we are using consumables ER 80S-B8 or optionally ER90S-B91.

I would like to request members who have experience welding with ER 90S-B91 (closely related to ER90S-B9) to share any necessary precautions or considerations that should be taken during welding.refere below we are taking care,

1.Preheat to 210 degree centigrade minimum.
2. Interpass 300 degree centigrade maximum.
3. What are other recommended?

Best regards,
Bilal Chauhadry,

Vishwas Keskar

unread,
Sep 15, 2025, 1:40:19 PMSep 15
to material...@googlegroups.com
Use ER90S-B8 
B91 is not a compatible consumable.


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion visit https://groups.google.com/d/msgid/materials-welding/CAOq7hqvpGAzaQ3urEHdwMRqn94bMZ-12BOsL0tkmmkLFLDFFNA%40mail.gmail.com.

venkateswara reddy Desireddy

unread,
Sep 15, 2025, 1:40:19 PMSep 15
to material...@googlegroups.com
Weld joint Post weld heating 100°C one hour should be maintained. 
Electric coil heating is preferred to maintain proper temperature.
Based on thickness PWHT to be done. 
To ensure weld quality go for helium leak test. 


From: material...@googlegroups.com <material...@googlegroups.com> on behalf of Ch Bilal jovinda <chbilal...@gmail.com>
Sent: Monday, September 15, 2025 8:09:58 PM
To: material...@googlegroups.com <material...@googlegroups.com>
Subject: [MW:35814] Material SA 335 P9 (P No. 5B) Welding with ER 80S-B8 or ER90S-B91
 
--

patni engineers

unread,
Sep 15, 2025, 10:50:12 PMSep 15
to material...@googlegroups.com
Dear Sir,

SA335 P9 is a highly weldable material. We have successfully completed a job for EIL using this material and have the relevant WPS PQR and PWHT documentation for P9.

We would be happy to share these with you if you are interested.

Regards,


Chandrakant
B.E Mech.
ASNT Level II RT/UT/PT/MPT/CSWIP
Patni Engineers. Mumbai. India
PED/2014/68/EU
welding shop AD2000/DIN EN ISO 3834
IBR Approved 

Factory Addreess- Pl Call 

Sankaran Sp

unread,
Sep 16, 2025, 1:35:50 PMSep 16
to material...@googlegroups.com
Dear friend
For wedding of this chrom & moly type steel 
Similar type composition consumable can be used 
Pre heat & post heating is essential
Interpass temperature to be maintained
Pwht also to be followed after welding.

Regards
Sankaran .sp 
Welding & metallurgy expert


--