Dear Sir,
We would like to know that, Our PQR Base Metal (SA 516 GR.70) thickness is 70mm with Impact, or PWHT.
What is the minimum or maximum base metal thickness range qualified.
As per ASME SEC.IX QW 451 Procedure Qualification thickness limit mentioned in Table QW.451.1 given.
5 to 200 mm.
But our Clinet approved WPS  in mentioned 16 to 200mm. Where mentioned ASME SEC.IX reference is mentioned range of base metal thickness.

Please clarify base metal thickness range 16 to 200mm.


With Best regards,
Mohammad Imran Khan
QA/QC Engineer

Chandra

unread,
Apr 7, 2016, 12:26:04 AM4/7/16
to material...@googlegroups.com
Dear Imran,

If you tested your PQR with impact test.
Please refer to the ASME sec IX 
QW 403.6 : says the minimum base metal thickness qualified is the thickness of the test coupon T or 5/8 inch. (16mm) whichever is less.

So your test specimen is 70mm, so the base metal thickness range in your WPS shall be from 16mm to 200mm.

If you never do impact test on your PQR. You can go in your wps from 5mm to 200mm thk base metal.



Best Regards,
Chandra
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAC_iqqAR2WuxK2aVs0_9OdBVyoyQU6haivR%3Dz4aZKK%2BEFng_KQ%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

jaya anil

unread,
Apr 7, 2016, 12:57:21 AM4/7/16
to material...@googlegroups.com
Hi,

In your case, you need to qualify another PQR with 6mm or less with impacts to have minimum Thickness range.

You need to support 2 PQRs for your job one which you have already qualified with 70 mm and other with lesser thick.

Thanks
Anil

Malusare Vijay

unread,
Apr 7, 2016, 4:08:51 AM4/7/16
to material...@googlegroups.com

Kindly refer QW 403.3

--