Thermocouple Quantity

129 views
Skip to first unread message

pradip kumar Sil

unread,
Jul 1, 2016, 4:32:22 AM7/1/16
to materials-welding
Dear Everybody,
How many thermocouple to be  attached in the weldment during Pwht  / During Preheating , we are following as per  Project Specification.

My Question is anywhere in the code/ Standard  is it mentioned ? Pls refer
Thanks in advance
Regards
Pradip  

Rogelio Alegre

unread,
Jul 1, 2016, 10:57:56 PM7/1/16
to material...@googlegroups.com
Hi Pradip 
My suggestion is AWS D.10.10/D10.10M: 1999(R2009) – Recommended. Practices for Local Heating of Welds in Piping and. Tubing.
Kind regards 
Sent from my iPhone
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAB%3DAs8kLFfRTB_R82axYxBN8dEJPvfpJhY%3Ddm2seXUp7wd3B4Q%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Sudalai Kannan

unread,
Jul 1, 2016, 11:00:09 PM7/1/16
to material...@googlegroups.com
Dear Pradip,

As per API minimum 2 thermocouple shall be used and it' will be increased based on the diameter of the weldment.

Thanks & regards,
M.Sudalai.

--

Jignesh Desai

unread,
Jul 1, 2016, 11:03:50 PM7/1/16
to Materials & Welding
You may get some detail in WRC Bulletin 452.

Normally for for ASME vessels, number & location of Thermocouple shall be in compliance with temperature variation during heating, cooling and holding time with respect to specified span of length.

Regds/Jignesh 

pgoswami

unread,
Jul 1, 2016, 11:47:04 PM7/1/16
to material...@googlegroups.com

Hi Pradip,

 

You may refer AWS D-10.10, Fig 12—14 for guidelines on circumferential joints. The guidance is provided from 6” dia pipe to 30” dia pipes, with multiple zones of control.

 

D 10.10 recommends both Monitoring and Control thermocouples. Control thermocouple/s to be placed right on the weld, while the monitoring thermocouples are to be placed at the edge if the soak band as well as at the edge of the heating band.

 

Figures from D-10.10 can’t be reproduced due to copyright issues.

 

Alternatively WRC -452 may also be followed. This document was written in line with AWS D10.10.

 

One thing to note, in case of discrepancies between your project specification  and Local PWHT codes(e.g AWS D-10.10), the project spec would be more binding. Advice is to get this issue resolved with the concerned welding/ metallurgical engineers and move forward.

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist ,
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

H-905-6799677, 905-9631505

C-905-9793232

 


To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/F76B7425-8933-48C4-8CA2-F931A1F55EA8%40yahoo.com.ar.

Yuvaraj Bhingare

unread,
Jul 2, 2016, 5:53:04 AM7/2/16
to material...@googlegroups.com

dear expert please send me material grade nd electrode combination

pradip kumar Sil

unread,
Jul 2, 2016, 5:53:04 AM7/2/16
to materials-welding
Dear Rogelio,

I already searched AWS D10.10 but i did not get any clear idea regarding how many thermocouple to be used during welding/ PWHT  in piping.

Regards,

 

José Juan Jiménez Alejandro

unread,
Jul 2, 2016, 5:53:04 AM7/2/16
to material...@googlegroups.com

You see Procedure for Postweld Heat Treatment UW-40 in ASME Section VIII Div. 1, referer yo Welding Resrarch Council (WRC).

Hareesh K V

unread,
Jul 2, 2016, 8:43:16 AM7/2/16
to materials-welding

Dear Sir,

To my knowledge none of the  code specified the same. It is based on experience and client specification you have to work.

Regards,

Hareesh K V
+91-8547859202