We work on material selection about column materials (shell, head, skirt). If we use A-516 Gr.70 material in this project, does it require heat treatment for repair on the column during maintenance?

Column Sections.jpg
Column Drawing.jpg

Production Properties : Sour Service , Distilation Column

Best Regards

TC Kwa

nepročitano,
5. svi 2020. 02:32:0205. 05. 2020.
u material...@googlegroups.com
Hi,

If it is for Sour service, PWHT shall be done, since material is A-516 Gr 70.
Thank you. 


Regards,

Ir. TC Kwa

+6012-3998739

Email: tc...@yahoo.co.uk

LinkedIn Profile : https://my.linkedin.com/in/tckwa 





--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/c8e5362b-3f5e-4fdc-912f-cc390d512800%40googlegroups.com.

José Juan Jiménez Alejandro

nepročitano,
5. svi 2020. 12:19:0005. 05. 2020.
u material...@googlegroups.com
The material 516 Gr 70 is a P1, you are mentioning that it is a repair, I suggest you check Table UCS-56-1 (b) (ASME Section VIII Div. 1), where the PWHT requirements for P1 materials appear, in ( b) it makes some exceptions to the PWHT based on the thickness of the material, if you exceed those thicknesses you will have to do the PWHT, but because it is a repair you also have to check the NB-23 and API 650 since from what I see in the drawing is a kit for the O&G Industry.
The Skirt I do not think it should carry PWHT since it is not a pressurized part.
Cheers!.



--

Ing. José Juan Jiménez Alejandro

Independent Consultant in Parts

and Pressure Equipment

SSI-TPI

Móvil +52 1 812 352 4606

Skype: jjjimeneza





George Dilintas

nepročitano,
9. svi 2020. 23:31:5509. 05. 2020.
u material...@googlegroups.com
In sour service there is a HIC risk. This risk is reduced if PWHT is done even the weld thickness is lower than the limits of UCS-56-1

--

atul khatri

nepročitano,
11. svi 2020. 01:48:4411. 05. 2020.
u material...@googlegroups.com
Refer Table 1 for NACE SP0472  for PWHT requirement and its exemption.

Thanks
Atul Khatri