Dear Experts

I need some information about standard method or test procedure which introduce testing on SAW flux to assure low hydrogen content.

For example when I have BS EN ISO 14174 / S A FB 1 65 AC H5 flux, How could I assure this is H5?

Regards
--
M. Shokri Arfaei
ASNT NDT Level III
International Welding Engineer





pgoswami

unread,
Sep 11, 2016, 11:34:36 PM9/11/16
to material...@googlegroups.com

Hi Meisam,

 

You need to trust on the certification provided by the consumable manufacturer. Typically all reputed SAW welding consumable manufacturers carry out wire flux classification test, along with which they need to carry out the test for diffusible hydrogen content also.

 

Look at ASME Sec II, Pt C-SFA 5.17 for typical guidelines( I find this to be better explained)

 

AWS standard for diffusible hydrogen content is: (AWS A4.3-93-2006),. Standard Methods for Determination of Diffusible Hydrogen Content of Martensitic, Bainitic, and Ferritic Steel Weld Metal . This process is quite tedious. Only knowledgeable labs who test welding consumables on a regular basis, are capable of doing. One needs to find out more details before proceeding with the welded samples.

 

Hope this clarifies your doubt. Read through the following document for more details.

 

Thanks
      


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAC8uMts2uhtD4ToPUH1D9QZWnOvaCfubxj_SugMdmVZtoKmnBA%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Bavaria_en_BF10MW.pdf

meisam shokri arfaei

unread,
Sep 13, 2016, 12:44:58 AM9/13/16
to material...@googlegroups.com
Dear Sir,

Thanks for your reply. 

I Had a look on AWS A4.3 and find that this standard is more compatible with SMAW. The length of the sample is too short for SAW also the run-out length for start and end of the weld, however the SAW process mentioned in that standard. 

Regards

On Mon, Sep 12, 2016 at 8:02 AM, pgoswami <pgos...@quickclic.net> wrote:

Hi Meisam,

 

You need to trust on the certification provided by the consumable manufacturer. Typically all reputed SAW welding consumable manufacturers carry out wire flux classification test, along with which they need to carry out the test for diffusible hydrogen content also.

 

Look at ASME Sec II, Pt C-SFA 5.17 for typical guidelines( I find this to be better explained)

 

AWS standard for diffusible hydrogen content is: (AWS A4.3-93-2006),. Standard Methods for Determination of Diffusible Hydrogen Content of Martensitic, Bainitic, and Ferritic Steel Weld Metal . This process is quite tedious. Only knowledgeable labs who test welding consumables on a regular basis, are capable of doing. One needs to find out more details before proceeding with the welded samples.

 

Hope this clarifies your doubt. Read through the following document for more details.

 

Thanks
      

From: materials-welding@googlegroups.com [mailto:materials-welding@googlegroups.com] On Behalf Of meisam shokri arfaei
Sent: Sunday, September 11, 2016 3:47 AM
To: materials-welding@googlegroups.com
Subject: [MW:25367] SAW flux with low hydrogen content

 

Dear Experts

 

I need some information about standard method or test procedure which introduce testing on SAW flux to assure low hydrogen content.

 

For example when I have BS EN ISO 14174 / S A FB 1 65 AC H5 flux, How could I assure this is H5?

 

Regards
--

M. Shokri Arfaei

ASNT NDT Level III

International Welding Engineer

 

 

 

 

 

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.

To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/!%26!AAAAAAAAAAAYAAAAAAAAAOT5XfyRhstKvyeqQRSrfFXCgAAAEAAAAEVn8ssFyzRHqLl%2BdNQTVrEBAAAAAA%3D%3D%40quickclic.net.

For more options, visit https://groups.google.com/d/optout.
Reply all
Reply to author
Forward
0 new messages