We have to carried out PQR for one of vendor using material IS 2062 Gr. E450  for a structural fabrication work in India. The welding process to be used is SMAW, GMAW,SAW.
I would like to know the correct for welding because very limited information is available about this steel.
         Vendor suggested below consumables to be used :
- SMAW : E9018-M
- GMAW : ER 90S-D2
- SAW : EA2+F8A2

         So, requesting to guide regarding same

Regards,
Atul Bharat Garad
Mob. No. 9702909716

james gerald

unread,
Apr 10, 2023, 11:16:10 PM4/10/23
to material...@googlegroups.com
It;s equivalent to ASTM A572 Gr.65Type 1 and SMTS is 80ksi and hence you can try a E8018M/G & ER 80S-D2 or recommended by the Vendor

Thanks & Regards

J.Gerald Jayakumar



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b29dd043-2803-453f-8fab-81b35948d567n%40googlegroups.com.

Vinay

unread,
Apr 15, 2023, 12:23:05 AM4/15/23
to material...@googlegroups.com

atulb...@gmail.com


--
Reply all
Reply to author
Forward
0 new messages