GM

The WPS which is qualified with P1 Gr.2 with Clad Alloy 825 will qualify to weld P1 Gr.2 with Clad Alloy 625 to equivalent or same material…? required separate qualification for P1 Gr.2 with Clad Alloy 625 ?.


thanks in advance for your's prompt reply.


Babu 

Karthik

unread,
Jan 15, 2020, 2:40:07 AM1/15/20
to Materials & Welding
Hi,
Inconel 625 is P.Number 43 and Inconel 825 is P.Number 45. So you can not use the WPS of P.No.45 to weld P.No.43. Please find below the extraction from Sec.IX

Inline image


Thanks& Regards,

 

(Karthik)

Karthikeyan.S

E-mail : karthi...@yahoo.com



--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/9a533821-faa6-473e-be7f-15a39c2ffcc6%40googlegroups.com.
Reply all
Reply to author
Forward
0 new messages