Hi Mr Anamul,
For qualification mentioned in below mail ,thickness qualified is unlimited. Refer para QW-452.1b.
Note that Para QW-404.30 cross refers para QW-452.1b for performance qualification by radiography.
For position qualification refer para QW-461.9.
The welder is qualified to weld flat position for size less than or equal to 24" pipes and flat & vertical position in size more than 24" pipes.
hope this clarifies you.
Best regards,
Padmasanker.s
Project quality coordinator,
Bilfal heavy industries ltd.
I the deposited thickness was 13 mm and over and he has deposited at least 3 layers then the range is not 2t but the maximum to be welded (restricted by the WPS)
best regards
Dr. Georgios Dilintas
Authorized Nuclear Inspector
Authorized Inspector Supervisor
I&F REGIONAL TECHNICAL MANAGER
BUREAU VERITAS HELLAS A.E - PIRAEUS GREECE
Tel: +30 210 40 63 113 /4 /5
Fax: +30 210 40 63 118
Cell: +30 69 44 64 62 04
anamulqc---19/01/2016 04:25:18---Dear Sir, We conducted welder qualification at Karbala Oil Refinery Project as per
From: anam...@gmail.com
To: Materials & Welding <material...@googlegroups.com>
Date: 19/01/2016 04:25
Subject: [MW:24126] Qualified thickness for welder
--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/b86d11c7-1ff9-4ee6-b63e-040e6aafcdbe%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.
This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com
Not clear answer?
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/OF33EABFCF.05BC7116-ONC2257F49.00369FB5-C2257F49.0036BBAE%40LocalDomain.