Dear Sirs, 

Pleas help me to Select electrode ? for AISI 4130 (70-75 Ksi) and API 5CT L80 Pipe materials to weld by SMAW. 

Using ASME IX Code.  

Thanks and Best Regards,
Ehab Ahmed

Venkatachalam Govindan

읽지 않음,
2019. 6. 12. 오전 11:55:5119. 6. 12.
받는사람 material...@googlegroups.com
Hi Ehab,
  1. E 10018-D2 - Electrode - SMAW
  2. ER 80S-D2 - FIller Wire - GTAW
You can use for SMAW first one.

Best Regards,

Venkat. G


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/20385728-b6dc-46fa-b65c-7fc06c8a7b47%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.


--
Venkatachalam Govindan
QHSE Lead / Trainer
(IRCA Registered Lead Auditor & API / CQI Practitioner)
+965 97604989, +919840502376 (
WhatsApp only)

Bien_ND

읽지 않음,
2019. 6. 18. 오전 5:59:1419. 6. 18.
받는사람 Materials & Welding
A5.5 E11018-M, easy to order.
Cooling rate control is important and PWHT to reduce stress.

Ehab Ahmed

읽지 않음,
2019. 7. 15. 오전 5:52:0119. 7. 15.
받는사람 Materials & Welding


On Wednesday, June 12, 2019 at 8:22:55 AM UTC+3, Ehab Ahmed wrote:
Dear Sirs, 

Pleas help me to Select electrode ? for AISI 4130 (70-75 Ksi) and API 5CT L80 Pipe materials to weld by SMAW. 

Using ASME IX Code.  PQR should Meet Requirement according to NACE MR0175 

Ehab Ahmed

읽지 않음,
2019. 7. 15. 오전 5:53:1119. 7. 15.
받는사람 Materials & Welding
Dear Mr. Venkat. G

Thanks for your support and i would like to be inform if selected electrode meet NACE MR-0175 and hardness limited to 23 Max HRC
during my search i found E8018-B2 or E8018-C3 more accurate for H2S or Sure Service.

**Last question if i can use this electrode for Root or i have to select another electrode for pipe Root.      


On Wednesday, June 12, 2019 at 6:55:51 PM UTC+3, Venkat QMR (IRCA, Lead Auditor)) wrote:
Hi Ehab,
  1. E 10018-D2 - Electrode - SMAW
  2. ER 80S-D2 - FIller Wire - GTAW
You can use for SMAW first one.

Best Regards,

Venkat. G


On Wed, Jun 12, 2019 at 8:22 AM Ehab Ahmed <elpop...@gmail.com> wrote:
Dear Sirs, 

Pleas help me to Select electrode ? for AISI 4130 (70-75 Ksi) and API 5CT L80 Pipe materials to weld by SMAW. 

Using ASME IX Code.  

Thanks and Best Regards,
Ehab Ahmed

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to material...@googlegroups.com.

Bestun Ahmed

읽지 않음,
2022. 6. 20. 오전 6:04:5722. 6. 20.
받는사람 Materials & Welding
Hello Sirs,
For the same issue Please can you gents Mr. Venkat and Mr. Ehad share the used WPS for this process.