Details of wleding grove and gap

49 views
Skip to first unread message

Pampanagouda Haraginadoni

unread,
Aug 11, 2023, 6:57:03 AM8/11/23
to material...@googlegroups.com
Dear Sir's
Can Anybody clear that for 10mm thickness plates how much root gap with back strip to be made as per ISO9692-1 and in this stanrd showing >16mm but it is 10mm plate so that i m doubt about this. 
so that can anybody help in this regard
image.png


H .PAMPANAGOUDA.PATIL| (CRS&I-SHOP) Vijayanagar Works | JSW Steel Limited
P.O. Vidyanagar  | Dist. Bellary  | Karnataka-583275 | India
Direct : +91 8395 243105
Cellphone: +91 9480694735
Email : pampanagouda...@jsw.in 
Website: www.jsw.in
P Print only when necessary |7 Switch off as you go |qRecycle always
#Better Everyday


Confidentiality Notice

The information  contained in this electronic message and any attachments to this message are intended  for the exclusive  use of the addressee(s)  and may contain  confidential  or privileged information. If you are not the intended recipient, please notify the sender at JSW  or  System Manager ( ad...@jsw.in ) immediately  and destroy all copies of this message and any attachments.  Recipients must check this email and its attachments  for the presence of viruses before downloading them. JSW Group accepts no liability for any damage caused by any virus transmitted by this email.

Vishwas Keskar Welding Manager WELDING

unread,
Aug 12, 2023, 5:21:57 AM8/12/23
to Materials & Welding
As I understand that ISO9692-1 is not specifying any root gap for 10mm  plate thickness welding. 
In that case following is suggested - 
The Plate bevel shall be 45-50 Deg 
Root opening with backing - 6-8 mm 
This will have access for full fusion 

Thanks 

Vishwas -IWE 