Tungsten Rod Query

29 views
Skip to first unread message

Vino Varghese

unread,
Sep 26, 2015, 7:47:36 AM9/26/15
to material...@googlegroups.com

Experts,

Which is the best Tungsten rod for welding CS or SS steel? What's the factors for choosing the right rod for welding? It is emphasised that for Aluminum welding, Zr-1 is a better option compared to Thoriated one. Is there any health hazard regarding the same and how does it affects the welding pool?

Hope to see your suggestion for my better understanding.

Thanks and Regards
Vino, Doha

pgoswami

unread,
Sep 26, 2015, 1:06:07 PM9/26/15
to material...@googlegroups.com, vinopv...@gmail.com
Hello, Vino,
 
Please see the attached document which will answers to all of your queries. Usually "Thoriated Tungsten" is most common for all DC welding involving all varieties of metals. Zirconiated is preferred for A.C power sources, which is ideal and most recommended for welding Aluminum and its' alloys.
 
Usually there's not much of health hazards involved with a change of Tungsten Electrode.
 
Thanks.
 
Pradip Goswami, P.Eng,IWE
Welding & Metallurgical Engineering Specialist
Hamilton, Ontario, Canada
 


From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of Vino Varghese
Sent: Saturday, September 26, 2015 6:49 AM
To: material...@googlegroups.com
Subject: [MW:23557] Tungsten Rod Query

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAM7oz7Cgy4462jUTGKWkSDy2dB%2B%3DieDUPQ9ynv49YiaAF4EBRg%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.
Guidelines for tungsten electrodes - TheFabricator.pdf

Kannayeram Gnanapandithan

unread,
Sep 27, 2015, 1:15:49 AM9/27/15
to materials-welding
In line with Goswami, For AC GTAW---- 0.5% Zr is the best if not available use Pure tungsten, do not use thoriated.
For DC GTAW  2% Cerium is best because 2% Thoriated is hazards to health while grinding/Sharpening( Radiation)

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY