Base metals qualified WPQT AWSD1.1

37 views
Skip to first unread message

Umar Rashid Makrani

unread,
Feb 20, 2017, 4:58:37 AM2/20/17
to material...@googlegroups.com
Hello peers
I could not find what is the base metals qualified range as per D1.1 
could someone help me, please ?
--
 
With Best Regards,
Umar Rashid Makrani, PMP® ,
 API653, NACE CIP-2, LEEA Registered Engineer.

anthony chundal

unread,
Feb 20, 2017, 5:13:44 AM2/20/17
to material...@googlegroups.com
You will get this in section -4 table- 4.2, 4.10, 4.11.

Thanks & Regards,
Anthony.

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJCSKyh3WQFAOsJv28jCtzQVNCLULhK5UzMP%2Bgzei0c%2B4YCBxw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

ECHARU

unread,
Feb 20, 2017, 10:09:58 PM2/20/17
to material...@googlegroups.com
For wps- table 4.2,
For welder qualifications - table 4.11

Maharaja Elavarasan

From: anthony chundal
Sent: ‎20-‎02-‎2017 13:13
To: material...@googlegroups.com
Subject: Re: [MW:26114] Base metals qualified WPQT AWSD1.1

To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAOi%3DZp8Uctd7d_02JCvHH22R92Dm5Hm1e8MO8iSOXAdFncViCg%40mail.gmail.com.

Umar Rashid Makrani

unread,
Mar 3, 2017, 9:19:30 PM3/3/17
to Materials & Welding
Dear Experts,
Thank you very much.
my question was not complete i appologies for that, However i appreciate for the answer. Table 4.11 shows dimensions and thickness limits only. The Table 4.12 was more informative for me. With that I understood that:
  • Base Metal is not an essential variable for WPQ.
  • A welder who is qualified for the F- Number Range may weld any metal in a qualified WPS using that F-number.
  • there is no concept of p number as in ASME BPV Section 9
Please advice if otherwise.

On Tuesday, February 21, 2017 at 6:09:58 AM UTC+3, aru ara wrote:
For wps- table 4.2,
For welder qualifications - table 4.11

Maharaja Elavarasan

From: anthony chundal
Sent: ‎20-‎02-‎2017 13:13
To: material...@googlegroups.com
Subject: Re: [MW:26114] Base metals qualified WPQT AWSD1.1

You will get this in section -4 table- 4.2, 4.10, 4.11.

Thanks & Regards,
Anthony.
On Mon, Feb 20, 2017 at 12:15 PM, Umar Rashid Makrani <firoz....@gmail.com> wrote:
Hello peers
I could not find what is the base metals qualified range as per D1.1 
could someone help me, please ?
--
 
With Best Regards,
Umar Rashid Makrani, PMP® ,

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CAJCSKyh3WQFAOsJv28jCtzQVNCLULhK5UzMP%2Bgzei0c%2B4YCBxw%40mail.gmail.com.