Ferrite % 4-8 of E309LMo

59 views
Skip to first unread message

SATISH SHAH

unread,
May 20, 2016, 10:51:28 PM5/20/16
to Materials & Welding
Dear Expert,

Let me know Ferrite 4 - 8 % is possible to obtain of Electrode 309LMo as weld condition.


Regards

SATISH SHAH

Mohd Siraj

unread,
May 21, 2016, 10:56:44 PM5/21/16
to Materials & Welding
How much did you get on PQR?.

ferrite depend on many other factor other than just filler wire.

dili...@gmail.com

unread,
May 24, 2016, 5:40:41 AM5/24/16
to Materials & Welding
The purpose of this filler metal is to avoid hot cracking. This is achieved by giving at least Ferrite no 5

Sent from my BlackBerry 10 smartphone.
From: SATISH SHAH
Sent: Σάββατο, 21 Μαΐου 2016 - 05:51
To: Materials & Welding
Subject: [MW:24816] Ferrite % 4-8 of E309LMo

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/8c7f5e73-c5e0-4c60-ab4f-92cb2537713b%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Vishwas Keskar Welding Manager Pune India

unread,
Jun 20, 2016, 7:06:55 AM6/20/16
to Materials & Welding
TYP 309 Mo will have higher ferrite @10-12 
check with consumable manufacturer 

Rajnish Dixit

unread,
Jun 20, 2016, 10:45:51 PM6/20/16
to material...@googlegroups.com
Dear Mr. Shah,

First you have to purchase electrodes as per the your specified requirment.

In addition to the above, for achieving this you have to take care for following:

1. No filing/ brushing/ grinding etc. should be done on welds before measuring ferrite %
2. Allow weld to cool in open air
3. The ferrite should be measured immediately after cooling of the welds

Best Regards,
Rajnish


--------------------------------------------
On Fri, 5/20/16, SATISH SHAH <sbdr...@gmail.com> wrote:

Subject: [MW:24816] Ferrite % 4-8 of E309LMo
To: "Materials & Welding" <material...@googlegroups.com>
Date: Friday, May 20, 2016, 3:49 PM

Dear Expert,

Let me know Ferrite 4 - 8 % is possible to obtain of
Electrode 309LMo as weld condition.


Regards

SATISH SHAH




George Dilintas

unread,
Jun 21, 2016, 10:26:52 PM6/21/16
to Meghanadh K
What is welded with? with other words: what are the base metals

2016-05-22 5:55 GMT+03:00 Mohd Siraj <mohd...@gmail.com>:
How much did you get on PQR?.

ferrite depend on many other factor other than just filler wire.
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.

For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis
Reply all
Reply to author
Forward
0 new messages