cladding of spherical surfaces by stellite

48 views
Skip to first unread message

Himan Nikdin

unread,
Apr 19, 2015, 11:42:40 PM4/19/15
to material...@googlegroups.com
Dear Experts;

My ball valve vendor claims that "it is not recommended to clad ball part of ball valve by stellite", I am looking for a reference to find is there any specific  limitation for this material.
The ball material is "SS316L".
If yes, is this limitation applicable for other stainless steel material like "13%Cr".

Thanks
Himan Nikdin

Venkatesan Mass tech

unread,
Apr 20, 2015, 4:59:02 AM4/20/15
to material...@googlegroups.com

Dear sir,
         please give the dimension of the ball valve size.

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/BLU180-W672B8F468DF26C214D739A9EE10%40phx.gbl.
For more options, visit https://groups.google.com/d/optout.

Tapasvi Lolla

unread,
Apr 21, 2015, 11:55:56 PM4/21/15
to material...@googlegroups.com
Hello Himan,

One of the main issues that can be encountered is the mismatch in thermal expansion properties when service temperature plays a role (mismatch can also play a role during solidification of clad if the cladding parameters are not crafully chosen) . In such instances cladding is actually good because, due to the dilution, it can create a gradual gradient in such properties and reduce the mismatch. But the dilution zone from the cladding process is known to form sigma phase (hard and brittle phase) at high temperatures. So my questions to you are:

1. What grade of Stellite is going to be cladded
2. What are the service temepratures like. 

Himan Nikdin

unread,
Apr 23, 2015, 3:27:28 AM4/23/15
to material...@googlegroups.com
Dear Sir

The sellite grade is 6, and the operating temperature is less than 100 C.

Regards,
Himan


Date: Tue, 21 Apr 2015 06:18:51 -0700
From: aceta...@gmail.com
To: material...@googlegroups.com
Subject: Re: [MW:23139] cladding of spherical surfaces by stellite