I am using IS 2062 Gr. A & B material for tank construction with A 106 Gr. B material for nozzles. Please let me know is clause number 5.7.4.2 of API 650 is applicable here? Shall I do PWHT for all opening connections (nozzles) NPS 12 or larger in nominal diameter?

hwj...@tce.co.in

unread,
Apr 14, 2015, 7:11:31 AM4/14/15
to makr...@gmail.com, material...@googlegroups.com

It is requested that the latest version of IS 2062 be referred to. There are no longer grades named after 'B'. Further the std. no longer supports steels meant for pressure vessels.  





your truly
H W JOSHI
ENGINEER MECHANICAL
TATA CONSULTING ENGINEERS LTD
MUMBAI - 400 083
TEL : 022 61148414



Makrand Sakpal <makr...@gmail.com>
Sent by: material...@googlegroups.com

14-04-2015 08:24


To
material...@googlegroups.com
cc
Subject
[MW:23080] IS 2062 Gr. A & B - PWHT for storage tank





Dear all,

I am using IS 2062 Gr. A & B material for tank construction with A 106 Gr. B material for nozzles. Please let me know is clause number 5.7.4.2 of API 650 is applicable here? Shall I do PWHT for all opening connections (nozzles) NPS 12 or larger in nominal diameter?

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to
materials-weld...@googlegroups.com.
To post to this group, send email to
material...@googlegroups.com.
Visit this group at
http://groups.google.com/group/materials-welding.
To view this discussion on the web visit
https://groups.google.com/d/msgid/materials-welding/5c8ca57c-6a15-427d-8b93-b4244f826957%40googlegroups.com.
For more options, visit
https://groups.google.com/d/optout.


----------------------------------------------------------------------------------------------------------
Information transmitted by this E-MAIL is intended only for the use of the addressee(s) and contains information that is privileged, confidential or exempt from disclosure under applicable law. If you are not the intended recipient or it appears that this mail has been forwarded to you without proper authority, you are notified that any use or dissemination and or copying of this email in any manner is strictly prohibited and you are requested to delete this e-mail immediately.
Communicating through e-mail is not secure and capable of interception and delays. Any one communicating with TATA Consulting Engineers Ltd., and / or its subsidiaries or associates or group companies by e-mail accepts the risks involved and their consequences.
While this e-mail has been checked for all known viruses, the addressee should also scan for viruses and notify the originator of e-mail.
---------------------------------------------------------------------------------------------------------

Asif Raza

unread,
Apr 14, 2015, 7:12:38 AM4/14/15
to material...@googlegroups.com

Yes dear it is applicable as IS 2062 is equivalent to A36, 2ndly PWHT is required for the NPS 12, the stress relief shall be 
carried out within a temperature range of 600°C – 650°C (1100°F – 1200°F) (see 5.7.4.3 for quenched and tempered materials) 
for 1 hour per 25 mm (1 in.) of shell thickness. The assembly shall include the bottom reinforcing plate (or annular plate) and the 
flange-to-neck weld. Also verify it from WPS requirement.

 