Dear to all,

I would like to ask you about the combination of pqr's

I have PQR A - 8mm (gtaw+smaw)
PQR B - 21.5mm (gtaw+smaw)
Both the pqr's were impact tested

now i want to make a wps using the 2pqr's as the thickness range 8mm to 43mm with impact requirements.

I require suggestions on this. Please give comments n valuable answers

Chandra
Welding Engineer


Best Regards,
Chandra

Lalu Rajendran

unread,
Mar 19, 2016, 8:01:15 AM3/19/16
to material...@googlegroups.com
Hi,
please refer the below extract QW-200.3 (f), and hope this will suffice.

Inline image 1

regards,
LALU


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/6F07097A-4544-4757-AC19-2334BE4464DD%40gmail.com.
For more options, visit https://groups.google.com/d/optout.

Gopi Krishna Banerjee

unread,
Mar 19, 2016, 11:06:27 PM3/19/16
to material...@googlegroups.com
Dear Sir.
  It is QW – 200.2 (f).
Thanks.
G. K.  Banerjee.

 

Chandra

unread,
Mar 20, 2016, 2:40:24 AM3/20/16
to material...@googlegroups.com
My thinking is QW-200.3(f) when impact test not require.
Must refer to QW-200.4(b) but reading that para, still confuses.
Could anyone suggest more???


Best Regards,
Chandra

On 19-Mar-2016, at 7:00 PM, Lalu Rajendran <lal...@gmail.com> wrote:

Hi,
please refer the below extract QW-200.3 (f), and hope this will suffice.

<image.png>

regards,
LALU

wilfred kojo

unread,
Mar 20, 2016, 5:19:11 AM3/20/16
to material...@googlegroups.com, Chandra
Though asme ix permit combination of two pqs to make one wps, yet that does not mean that 2 pqr could be indiscriminately be combined. You can combine 2 pqr if there is overlap in essential and supplementary essential variables of the 2 pqr. For example the requires reduction of 55ºC as essential variable and increase of more than 55ºC in preheat as supplementary essential variable. 
If your case you pqr A preheat = 50ºC , then range qualified = 5- 105 and 
Pqr B preheat  = 170 , then range allowed = 115 - 225.
Since there is overlap between the two examples,  then both can not be combined. 
Note,  the figures stated above are just examples not real figures. 

Wilfred Kojo ( AWS CWEng )


On Sun, 20 Mar, 2016 at 7:35 am, Chandra

George Dilintas

unread,
Mar 23, 2016, 1:21:22 AM3/23/16
to Meghanadh K
you can not exceed the base metal thickness qualified with the PQRB

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/6F07097A-4544-4757-AC19-2334BE4464DD%40gmail.com.
For more options, visit https://groups.google.com/d/optout.



--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

Lu, Feng

unread,
Mar 24, 2016, 12:08:14 PM3/24/16
to Meghanadh K

If the code governing the job is B31.3, then the qualified range shall be T/2 ~ (T+1/4”).  In this specific case, PQR A qualified 4mm ~ 14mm and PQR B qualified 11mm ~ 28mm, so your range shall be 4mm ~ 28 mm.

 

 

Zachry Group Logo

Feng Lu, Ph.D.
Metallurgy and Welding Engineer

Zachry Industrial, Inc.
527 Logwood
San Antonio, TX 78221

l...@zachrygroup.com
Office: 210.588.7818
Cell: 512 797 5777
Fax: 210.588.5037
www.ZachryGroup.com

This e-mail may contain confidential and privileged material for the sole use of the intended recipient. Any review, use, distribution or disclosure by others is strictly prohibited. If you are not the intended recipient (or authorized to receive for the recipient), please contact the sender by reply e-mail and delete all copies of this message.

dili...@gmail.com

unread,
Mar 25, 2016, 12:23:49 PM3/25/16
to Lu, Feng
The latest edition of 31.3 has no specific requirements besides those of ASME IX

Sent from my BlackBerry 10 smartphone.
From: Lu, Feng
Sent: Πέμπτη, 24 Μαρτίου 2016 - 18:08
To: Meghanadh K
Subject: RE: [MW:24572] Reg: combination of 2pqr's make a wps

Reply all
Reply to author
Forward
0 new messages