Bruscato X factor

86 views
Skip to first unread message

Pravin Poornachandran

unread,
Nov 15, 2022, 10:29:37 PM11/15/22
to 'Bijay' via Materials & Welding
Dear Expert,

Can anyone share or explain how to calculate Bruscato X factor for Gr.22 grade especially on welding consumable chemical composition.

Mind sharing any supporting document or article on how to calculate X factor. 

In my knowledge, X factor is trace elements which usually not guaranteed by manufacturer and it’s unintentionally added such as Sn, Sb, As etc.

Best regards,
Pravin 

Vishwas Keskar

unread,
Nov 16, 2022, 10:17:54 PM11/16/22
to material...@googlegroups.com
Refer API 934 A 
You can details 


Sent from my iPhone

On 16-Nov-2022, at 8:59 AM, Pravin Poornachandran <htcis...@gmail.com> wrote:

Dear Expert,
--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CADDyn7eDnamAySywpAepJJvDTzjvqr3C7bOJ1OQGP9cr3S5zug%40mail.gmail.com.

Anilkumar G

unread,
Nov 16, 2022, 10:18:27 PM11/16/22
to material...@googlegroups.com
Please check API 934-A

--

Prakash Hegde

unread,
Nov 16, 2022, 11:34:52 PM11/16/22
to material...@googlegroups.com

X-factor is a calculation, or formula, that measures a weldment's resistance to temper embrittlement, a brittleness or loss of toughness that occurs when the weldment is held (or slowly cooled) through a temperature range of approximately 850 to 1,100 degrees F.04-May-2010

On Thu, 17 Nov 2022 at 10:02, Prakash Hegde

Bruscato X factor (2).

J=(Mn + Si)(P + Sn) x104 (in wt %), has been applied to parent steels and 

weld metals.

X=(10P + 5Sb + 4Sn + As)/100 (in ppm), is applied to weld metals.



Prakash Hegde

unread,
Nov 16, 2022, 11:34:56 PM11/16/22
to material...@googlegroups.com

Bruscato X factor (2).

J=(Mn + Si)(P + Sn) x104 (in wt %), has been applied to parent steels and 

weld metals.

X=(10P + 5Sb + 4Sn + As)/100 (in ppm), is applied to weld metals.