Impact test- minimum thk requirement

2,262 views
Skip to first unread message

victor george

unread,
May 22, 2013, 6:33:28 AM5/22/13
to material...@googlegroups.com, Arul prakash
Hi Experts,
 
Please explain what is the minimum thickness requirement of impact test.
 
Material: A790 S31803 pipe
Size: 1/2' Sch 80 (WT- 3.73mm)
Sour service
 
 
Question: Is it possible to do impact test on 3.73 thk?
 
 
Best Regards,
DV.George
 

bruce alavi

unread,
May 22, 2013, 6:39:01 AM5/22/13
to material...@googlegroups.com, Arul prakash
Impact testing is not related to min or max materials thickness it is as per the project and code specification, check your project and design requirements
 
Very Best Regards
Behrooz Alavi

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 


james gerald

unread,
May 22, 2013, 6:54:40 AM5/22/13
to material...@googlegroups.com
Impact test not required/cannot be performed if the thickness is below 2.5mm.
 
Check with Metallurgy Lab whether they can machine your sample with thickness 3.73mm and perform Impact.
 
If yes, then Impact test need to be performed at -46/-50degC for Duplex.
 
Thanks & Regards

J.Gerald Jayakumar
00968-99438165
From: victor george <dvge...@gmail.com>
To: material...@googlegroups.com
Cc: Arul prakash <r.arul...@gmail.com>
Sent: Wednesday, May 22, 2013 2:33 PM

Subject: [MW:17738] Impact test- minimum thk requirement

Rajaram chandrasekaran

unread,
May 22, 2013, 7:25:33 AM5/22/13
to material...@googlegroups.com, Arul prakash, dvge...@gmail.com

dear experts
you can do impact test on your material 1/2" sch 80_3.73mm thickness by making the impact  specimen sample as 10 X 2.5 X 55 as per astm a370 and astm e23 or by making the specimen thickness as more than 80% of the material thickness

regards
rajaram.c

--

Ramin Kondori

unread,
May 22, 2013, 10:50:05 AM5/22/13
to material...@googlegroups.com
Dear Victor:

In our project we have similar requirements for Duplex and Super Duplex as James mentioned (regardless of thickness) where it requires impact test at -46 degC and results should demonstrate average of minimum 27J and no result less than 20J).

Regards
Ramin Kondori
Sr. QA/QC Engineer
SINOPEC

r.ko...@petroyada.com
+98-2123592322
+98-9132150320

K E Satyanarayana

unread,
May 22, 2013, 11:55:56 PM5/22/13
to material...@googlegroups.com
Hi
yes it is possible upto 2.5 mm thk.
> --
> To post to this group, send email to material...@googlegroups.com
> To unsubscribe from this group, send email to
> materials-weld...@googlegroups.com
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google Groups
> "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send an
> email to materials-weld...@googlegroups.com.
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
>


--
*Best Regards,*
**
*K.E.SATYANARAYANA*
*SURVEYOR*
*BUREAU VERITAS INDIA PVT. LTD.*

kannayeram gnanapandithan

unread,
May 22, 2013, 11:51:58 PM5/22/13
to material...@googlegroups.com
2/3 of 27 joules is also acceptable in some codes
Pandithan
welding consultant

On 5/22/13, Ramin Kondori <ramink...@gmail.com> wrote:
> *Dear Victor:*
>
> In our project we have similar requirements for Duplex and Super Duplex as
> James mentioned (regardless of thickness) where it requires impact test at
> -46 degC and results should demonstrate average of minimum 27J and no
> result less than 20J).
>
> Regards
> *Ramin Kondori*
> *Sr. QA/QC Engineer
> *
> *SINOPEC*
>
> r.ko...@petroyada.com
> +98-2123592322
> +98-9132150320
>
>
> On Wed, May 22, 2013 at 3:24 PM, james gerald <gerr...@yahoo.com> wrote:
>
>> Impact test not required/cannot be performed if the thickness is below
>> 2.5mm.
>>
>> Check with Metallurgy Lab whether they can machine your sample with
>> thickness 3.73mm and perform Impact.
>>
>> If yes, then Impact test need to be performed at -46/-50degC for Duplex.
>>
>> Thanks & Regards
>>
>> J.Gerald Jayakumar
>> 00968-99438165
>> *From:* victor george <dvge...@gmail.com>
>> *To:* material...@googlegroups.com
>> *Cc:* Arul prakash <r.arul...@gmail.com>
>> *Sent:* Wednesday, May 22, 2013 2:33 PM
>> *Subject:* [MW:17738] Impact test- minimum thk requirement

victor george

unread,
May 23, 2013, 12:17:47 AM5/23/13
to material...@googlegroups.com, Arul prakash, Venu Ragu
Thanks Gents.
It is very clear that impact test shall be performed up to 2.5mm thk.
 
Appreciate all your valuable guidance.
 
Best Regards,
Victor.

zubair

unread,
Oct 15, 2015, 4:01:11 AM10/15/15
to Materials & Welding
Dear ramin which code and section you refer -46 Cdeg,


Please elavorate ..

Harish Kannepalli

unread,
Oct 15, 2015, 4:19:55 AM10/15/15
to material...@googlegroups.com
For this diameter and thickness, it is not possible to perform  impact test.

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
 
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
For more options, visit https://groups.google.com/groups/opt_out.
 
 



--
Regards,
Mr. Harish.

Devin

unread,
Oct 15, 2015, 5:09:08 AM10/15/15
to material...@googlegroups.com, material...@googlegroups.com
George
sub-size impact test specimen could be used when  full sized specimen is not possible due to the thk of the weldment. But usually impact requirement is required only when the thk of production metal exceeds 16mm. 
Hope it helps.

Elshan Feyzullayev

unread,
Oct 15, 2015, 6:11:03 AM10/15/15
to material...@googlegroups.com
Hi DV George

The charpy requirements starts from 5 mm and above. Below 5 mm is not required as per ASTM A370  which is Standard Test Methods and Definitions for Mechanical Testing of Steel Products page 5 Note 7 2003 publication.  

On the other hand example 5 section 7 in EEMUA 153 which is SUPPLEMENT TO ASME B31.3 states as follows: 

"""""7 BS 3603, Charpy V-notch impact testing at low temperature BS 3603 : 1991 Sec. 12.2.3 states that impact testing shall not be carried out on tubes less than 6 mm thick. For the particular example in which a nominal wall thickness of 5.6 mm is specified, impact testing will not be carried out. However impact values may be assumed as those given for thicker material supplied to the same specification. """"" 

Also most of project specifications don't require charpy test below 6 mm.  Hence, in your case the impact test is not required. I think this clarifies your doubt.  

Best regards Elshan.

________________________________
> Date: Thu, 15 Oct 2015 12:11:43 +0400
> Subject: Re: [MW:23717] Impact test- minimum thk requirement
> From: harishka...@gmail.com
> To: material...@googlegroups.com
>
> For this diameter and thickness, it is not possible to perform impact test.
>
> 2013-05-22 14:33 GMT+04:00 victor george
> Hi Experts,
>
> Please explain what is the minimum thickness requirement of impact test.
>
> Material: A790 S31803 pipe
> Size: 1/2' Sch 80 (WT- 3.73mm)
> Sour service
>
>
> Question: Is it possible to do impact test on 3.73 thk?
>
>
> Best Regards,
> DV.George
>
>
> --
> To post to this group, send email to
> To unsubscribe from this group, send email to
> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
>
> The views expressed/exchnaged in this group are members personel views
> and meant for educational purposes only, Users must take their own
> decisions w.r.t. applicable code/standard/contract documents.
> ---
> You received this message because you are subscribed to the Google
> Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send
> an email to
> For more options, visit https://groups.google.com/groups/opt_out.
>
>
>
>
>
> --
> Regards,
> Mr. Harish.
>
> --
> You received this message because you are subscribed to the Google
> Groups "Materials & Welding" group.
> To unsubscribe from this group and stop receiving emails from it, send
> an email to
> To post to this group, send email to
> Visit this group at http://groups.google.com/group/materials-welding.
> To view this discussion on the web visit
Reply all
Reply to author
Forward
0 new messages