My question is In after Tubesheet Bonding PWHT required or Not?

Base Material : SA 516 GR 70. (Thk : 45 mm )
Bonding Material : SA 240 GR 316. (Thk:5mm)

Tubesheet Dia : 3000 mm

( Note : Bonding plate SS 316 : 1 No joint on base material)

Regards,
Ankit Patel
8140255303.

George Dilintas

unread,
Dec 2, 2020, 10:30:20 PM12/2/20
to material...@googlegroups.com
What do you mean by bonding

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALR-PuwRp0-NoHz6KXB6-4Y3tkTKmaB4pJxtF8HhM8ctpf3EtA%40mail.gmail.com.


--
Dr. Georgios Dilintas,
Dipl. Ing. In Aeronautic and Space Engineering
Ph.D in Mechanics of Solids - Computational Mechanics
A.I.S, A.N.I, IRCA Lead Auditor
Welding, Stress Analysis, Corrosion, QA/QC, Failure Analysis, Risk Analysis

udaya bhaskar

unread,
Dec 3, 2020, 12:34:04 AM12/3/20
to material...@googlegroups.com
Not Required PWHT For check bonding.
NDT required for check bonding

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CALR-PuwRp0-NoHz6KXB6-4Y3tkTKmaB4pJxtF8HhM8ctpf3EtA%40mail.gmail.com.


--
With Regards

Udaya bahaskar.D

udaya bhaskar

unread,
Dec 3, 2020, 12:34:04 AM12/3/20
to material...@googlegroups.com
Hello Mr. Ankith,
Please refer  for your clarification: PART UCL REQUIREMENTS FOR WELDED PRESSURE VESSELS CONSTRUCTED OF MATERIAL WITH CORROSION RESISTANT INTEGRAL CLADDING, WELD METAL OVERLAY CLADDING, OR APPLIED LININGS 

--

Patel Ankit

unread,
Dec 3, 2020, 12:34:07 AM12/3/20
to material...@googlegroups.com
Yes sir,

After Bonding PWHT required or not??

Kannayeram Gnanapandithan

unread,
Dec 3, 2020, 1:33:30 AM12/3/20
to materials-welding
is it explosive bonding

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015,
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


Patel Ankit

unread,
Dec 3, 2020, 6:37:16 AM12/3/20
to material...@googlegroups.com
Yes Sir,
It is explosive Bonding.

udaya bhaskar

unread,
Dec 3, 2020, 6:37:18 AM12/3/20
to material...@googlegroups.com
Mr.Patel, Doesn't require any PWHT after explosive cladding.  
if the customer wants you can, otherwise not.


Nithin Joseph

unread,
Dec 4, 2020, 10:27:04 PM12/4/20
to material...@googlegroups.com
When plate is bonded by explosion. The shape of the plate is disturbed, resulting in stresses and higher hardness. In order to straighten it up, it is always recommended to do a stress relieving heat treatment. It is nowhere specified, but to avoid issues during straightening and control hardness. 

--
Regards,
Nithin Joseph Dsilva

Patel Ankit

unread,
Dec 4, 2020, 11:30:07 PM12/4/20
to material...@googlegroups.com
Dear Sir,

If you say that stress receiving process required. My WPS also qualified with PWHT (SR) Process for SS 316 plate welding.

Pl. Suggest me.


Regards,
Ankit Patel

George Dilintas

unread,
Dec 7, 2020, 6:28:20 AM12/7/20
to material...@googlegroups.com
Could you send a sketch of the joint?
You question is not clear

Prasad Ghanekar

unread,
Dec 7, 2020, 10:39:55 PM12/7/20
to material...@googlegroups.com
Refering to SA264
HT is not mandatory for cladding process.
It's suplimentory requirement.

Prasad G.

james gerald

unread,
Dec 8, 2020, 3:46:03 AM12/8/20
to material...@googlegroups.com
Please provide below details.

1. Design Code.
2. Type of cladding like explosive cladding/cold rolling/weld metal overlay(electroslag strip/SAW strip/Laser)

Thanks & Regards

J.Gerald Jayakumar



Patel Ankit

unread,
Dec 11, 2020, 4:53:23 AM12/11/20
to material...@googlegroups.com
Dear Sir,

Construction code ASME SEC VIII Div 1.
Explosive Bonding.

Regards,
Ankit Patel

james gerald

unread,
Dec 16, 2020, 1:03:23 AM12/16/20
to material...@googlegroups.com
Dear Ankit,

Normally Explosive Bonding will be performed at Plate Mill and any Heat Treatment if required will be performed at Mill and covered via the MTC.

SS 316 clad plates fall under SA 264 (ASME Sec.IIA). According to the same for Explosive bonding, the clad plate shall be subjected to solution Annealing and the substrate base plate carbon steel Heat Treated to the Material standard separately  prior to Explosive Bonding and can be checked in the MTC.

Thanks & Regards

J.Gerald Jayakumar


Kannayeram Gnanapandithan

unread,
Dec 17, 2020, 3:07:59 AM12/17/20
to materials-welding
before bonding, CS shall be PWHT due to one joint, NDE cleared and Explosive bonding. with these procedure no PWHT required after bonding, otherwise required, Ref UCL-34

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,