Its will come under inclusion
will not come any separate criteria.




என்றும் அன்புடன்,

Best regards,

RAJAVARMAN SELVARAJ

+971561895584



On Wed, Jul 22, 2020 at 12:28 PM 'Dinesh' via Materials & Welding <material...@googlegroups.com> wrote:
Dear all experts,

Do you anybody aware about Filler wire inclusion(Filler cut) in GTAW.
In B31.3,nothing says.

Kindly share you ideas please.


--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/ffeecbcc-b1d2-48d9-8b0c-b62b863c3265n%40googlegroups.com.

Yahoo Mail

unread,
Jul 27, 2020, 12:10:41 AM7/27/20
to 'Dinesh' via Materials & Welding
During GTAW welding, filler wire in small bits gets dislodged from the main stem, falls 
back un-fused at the root. 
They call it as an un-melted filler wire or filler cut. This could happen,
1. If the welder uses reduced gap or un-focused arc, filler wire overheats, cut off from 
    the main stem un-melted and gets lodged at the root.
2. This can also happen if the welder uses more current or increased travel speed or the 
    arc gap is more.
3. It is considered as a defect and repaired. 

C Sridhar.
---------------------------------------------------------------------------------------------------------------------------------
 

in...@pieper-qsi.nl

unread,
Jul 27, 2020, 12:10:52 AM7/27/20
to 'Yahoo Mail' via Materials & Welding

Beste lezer,

U stuurde mij een e-mail. Dit is een automatisch antwoord daarop. Op dit moment ben ik op vakantie. Zodra ik weer aanwezig ben, stuur ik u zo snel mogelijk een reactie.

Met vriendelijke groet,
Herman Pieper

Pieper QSI

Reply all
Reply to author
Forward
0 new messages