Dear all,

 In our district cooling CS ( ASTM A106 Gr,B) pipeline project, pipe wall thickness is from 3.2 mm to 20.62 mm.  and our WPS is qualified and now we have to conduct welder qualification test.So what is the minimum   test coupon  thickness we should select so that welder can weld upto 20.62 mm thickness pipe during production.

WPS Details:

Welding process: GTAW & SMAW

Base metal thickness range : 5 - 22 mm

Weld metal groove for GTAW ; 6mm and SMAW - 16 mm



Prince C Thomas

K M JIJILAL

unread,
Jul 28, 2015, 12:23:42 AM7/28/15
to material...@googlegroups.com
Dear P C T,

You can select 6"  SCH 80/XS  (t=10.97 mm)
or
8"  SCH 80/XS  (t=12.7 mm) pipe test coupons for this purpose.

JijiLal K.M.,Welding Engineer,
Al banna Engineering LLC.
BPCL Kochi refinery expansion project.

Jiji Lal K M

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/0fdce533-3131-4418-bec0-6f0cef76fb24%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

Biplab Pal

unread,
Jul 28, 2015, 12:25:26 AM7/28/15
to materials-welding
Dear Prince,
It should be either 10.31mm or any thickness with 3 layer.

Regards
Biplab Pal

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/0fdce533-3131-4418-bec0-6f0cef76fb24%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.



--
Thanks & Regards
Biplab Pal
Welding Inspector
E-mail:   bipla...@gmail.com
 
Information in this email and any attachments is confidential and intended solely for the use of the individual(s) to whom it is addressed or otherwise directed. Please note that any views or opinions presented in this email are solely those of the author and do not necessarily represent those of the Company. Finally, the recipient should check this email and any attachments for the presence of viruses. Myself accepts no liability for any damage caused by any virus transmitted by this email.
 

george....@gr.bureauveritas.com

unread,
Jul 28, 2015, 5:48:02 AM7/28/15
to Prince C thomas
Your thickness divided by 2

Sent from my BlackBerry 10 smartphone.
From: Prince C thomas
Sent: Τρίτη, 28 Ιουλίου 2015 - 06:10
To: Materials & Welding
Subject: [MW:23220] reg: Test coupon thickness range

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at http://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/0fdce533-3131-4418-bec0-6f0cef76fb24%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

This message contains confidential information. To know more, please click on the following link: http://disclaimer.bureauveritas.com

Adriaan Stoltz

unread,
Jul 28, 2015, 10:25:35 AM7/28/15
to material...@googlegroups.com

Good day Mr Thomas. Dr George is correct. Please note however that your WPS does not cover you to weld  3.22mm up 4.99mm.

Nandesh Kumar

unread,
Jul 28, 2015, 11:49:37 PM7/28/15
to material...@googlegroups.com
Prince,

Input your variables here and know the range:

http://www.gowelding.com/wp/calc3.htm

ವಂದನೆಗಳೊಂದಿಗೆ / Best regards,

Nandesh Kumar Arasappa

P.S. : Please don't print this e-mail unless you really need to.

--------------------------------------------
On Tue, 28/7/15, Prince C thomas <prince...@gmail.com> wrote:

Subject: [MW:23220] reg: Test coupon thickness range
To: "Materials & Welding" <material...@googlegroups.com>
Date: Tuesday, 28 July, 2015, 12:13 AM
Reply all
Reply to author
Forward
0 new messages