Dear Experts,

We are doing pipeline  project for international client at UAE. We have completed around 400 joints(10 inch-11.1 mm) at site on conditional PQR( Except SSC/SOHIC  testing) as per NACE MR-0175/ISO 15156

Now the PQR test conducted for the SSC test and SOHIC test.

But the test lab informed that linear indication was observed in two test specimen after 30 days SSC test.

Now the client instructed to go more etching the surface and macroscopic examination.

Please suggest any acceptance criteria and resolution. Failure of the test will result huge impact on the 400 welded joints. Please suggest.

Pipeline Material:API 5L Gr.B X-60 as per shell standards.


Kalemullah
UAE-0569902364
 

Get your own FREE website, FREE domain & FREE mobile app with Company email.  
Know More >

pgoswami

unread,
Apr 13, 2016, 1:18:11 PM4/13/16
to material...@googlegroups.com, qama...@rediffmail.com

Hi Kalemullah,

 

MR-0175/ISO 15156 specifies that SSC/SOHIC testing should be done as per NACE TM-0177.This testing requirements are quite severe. You need to go through the results and try to seek the proper resolutions.

 

SOHIC testing on the PQR was originally called for in your project specifications??

 

Appreciate your response.

 

 

Thanks.

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist & Consultant.
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

 


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/20160413160528.13286.qmail%40f4mail-235-76.rediffmail.com.
For more options, visit https://groups.google.com/d/optout.

mohamed kalemullah

unread,
Apr 17, 2016, 10:45:50 AM4/17/16
to material...@googlegroups.com, pgoswami
"SSC test including SOHIC test to be conducted on the additional test specimen" as per project specification.

Remaning tests like Tensile,Macro,Hardness,Impact are all accepted.

Now we need any change in WPS or to go for the retest(30 days + PQR preparation). we have used BOHLER welding electrodes tested earlier for SSC test.


Please give your suggestion to proceed further.

Thanks lot.




From: "pgoswami" <pgos...@quickclic.net>
Sent: Wed, 13 Apr 2016 22:47:20
To: <material...@googlegroups.com>
Cc: <qama...@rediffmail.com>
Subject: [MW:24686] 24682] SSC test acceptance limit.

Hi Kalemullah,

MR-0175/ISO 15156 specifies that SSC/SOHIC testing should be done as per NACE TM-0177.This testing requirements are quite severe. You need to go through the results

SOHIC testing on the PQR was originally called for in your project specifications??

Appreciate your response.

Thanks.

Pradip Goswami, P.Eng,IWE
IndependentWelding & Metallurgical Engineering Specialist & Consultant.
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com


From: qama...@rediffmail.com [mailto:qama...@rediffmail.com]
Sent: Wednesday, April 13, 2016 12:05 PM
To: material...@googlegroups.com
Subject: [MW:24682] SSC test acceptance limit.


Dear Experts,

We are doing pipeline project for international client at UAE. We have completed

Now the PQR test conducted for the SSC test and SOHIC test.

But the test lab informed that linear indication was observed in two test specimen after 30 days SSC test.

Now the client instructed

Please suggest any acceptance criteria and resolution. Failure of the test will result huge impact on the 400 welded joints. Please suggest.

Pipeline Material:API 5L Gr.B X-60 as per shell standards.

Kalemullah

UAE-0569902364


Get your own FREE website, FREE domain & FREE mobile app with Company email.

Know More >

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational applicable code/standard/contract documents.

To view options views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.

Reply all
Reply to author
Forward
0 new messages