QW 404.12

86 views
Skip to first unread message

prem_nautiyal26

unread,
Oct 9, 2016, 9:30:21 AM10/9/16
to materials-welding

A WPS/PQR is qualified with ER 316L for corrosion resistant overlay as per ASME SEC IX.
welding process is GTAW.

Can this procedure be used for a welding procedure of ER 310 overlay.

Base material P No. are same.

ASME SEC IX QW 404.12 FOR change in filler metal classification is blank.

Regards

Prem Nautiyal 



Sent from my Samsung Galaxy smartphone.

Himan Nikdin

unread,
Oct 12, 2016, 4:59:25 AM10/12/16
to material...@googlegroups.com
I don't think so, Check A No..

Sent from my iPhone
--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/g4m33nfv05gtdps7ppoc3772.1476006551118%40email.android.com.
For more options, visit https://groups.google.com/d/optout.

Prakash Hegde

unread,
Oct 12, 2016, 5:00:34 AM10/12/16
to material...@googlegroups.com
Hi!
No you can not use this PQR  as AWS/UNS No of each category of SS No and A no as per QW404.37 is essential
Regards
Hegde P.B.


Kannayeram Gnanapandithan

unread,
Oct 12, 2016, 11:48:49 AM10/12/16
to materials-welding

A no for 310 weld metal is 9


--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-welding+unsubscribe@googlegroups.com.
To post to this group, send email to materials-welding@googlegroups.com.

Vishwas Keskar Welding Manager Pune India

unread,
Oct 12, 2016, 11:58:39 PM10/12/16
to Materials & Welding, prem_na...@yahoo.com
NEW PQR is required as A NO OF ER316L is 8  and ER310 is 9 