Dear All,

   In my project Slip on flange to Pipe We have 7 mm gap .. Pipe have ovality 

Now my client saying to us to do buttering at flange at machining 

If we do buttering at flange its allowed in the code book 

Please guide me

Best regards
Sankar.k

Jim Price

unread,
Feb 23, 2016, 7:46:28 AM2/23/16
to material...@googlegroups.com

 

Please see UW 42 of ASME Section VIII Div 1.  A butt welding procedure is enough for buttering.

 

UW-42 SURFACE WELD METAL BUILDUP
Construction in which deposits of weld metal are applied to the surface of base metal for the purpose of:
(a) restoring the thickness of the base metal for strength consideration; or
(b) modifying the configuration of weld joints in order to provide the tapered transition requirements of UW-9(c)
and UW-33(b) shall be performed in accordance with the following rules:
(1) A butt welding procedure qualification in accordance with provisions of Section IX must be performed for
the thickness of weld metal deposited, prior to production welding.
(2) All weld metal buildup must be examined over the full surface of the deposit by either magnetic particle
examination to the requirements of Appendix 6, or by liquid penetrant examination to the requirements of Appendix 8.
When such surface weld metal buildup is used in welded joints which require full or spot radiographic examination,
the weld metal buildup shall be included in the examination.

 

Reference Appendix 6 Section VIII Div 1

Buildup QW202.3

Thickness QW451.1

 

Best Regards

 

 

Jim Price | Welding Engineer, CWI

Direct:  320.7463439 | Fax: 417-862-5564

jimp...@polarcorp.com

cid:image001.jpg@01D0E005.E9837830

--
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/97c5d7b8-713a-4625-afc8-9bcbd722e7a2%40googlegroups.com.
For more options, visit https://groups.google.com/d/optout.

sankar bombay

unread,
Feb 24, 2016, 10:37:31 PM2/24/16
to material...@googlegroups.com
It's for butt joint what about flange inside buttering to reduce gap between pipe and flange (slip on flange ) ... 

There is any heat treatment required for flanges 

Thanks for your reply

Best regards
Sankar

For more options, visit https://groups.google.com/d/optout.


--
shankar

dili...@gmail.com

unread,
Feb 25, 2016, 1:23:15 AM2/25/16
to sankar bombay
I would help if you send a drawing or a sketch

Sent from my BlackBerry 10 smartphone.
From: sankar bombay
Sent: Πέμπτη, 25 Φεβρουαρίου 2016 - 05:37
Subject: Re: [MW:24366] Flange Buttering

Lakshman

unread,
Feb 25, 2016, 1:23:31 AM2/25/16
to material...@googlegroups.com

Hi Friend,

Instead of flange buttering and re machining you can go for a layer build up on the pipe, and particularly for your case pipe has ovality, then as per the gap positions you can deposit single layer or multiple layer and have a proper grinding to give proper fitup to flange.

 

 

Thanks & Regards,

Lakshman Kumar B,

+91 9440031459.

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of sankar krishnan
Sent: Tuesday, February 23, 2016 11:08 AM
To: Materials & Welding
Subject: [MW:24361] Flange Buttering

 

Dear All,

--

sankar bombay

unread,
Feb 25, 2016, 4:51:38 AM2/25/16
to material...@googlegroups.com
Hai brother, 

  It's correct I have suggested same .. but my client told me to do buttering inside flange to close gap between pipe and flange due to ovality 

 Now my question is there is any code allow to do buttering at flange 

If yes means .. there is heat treatment necessary for that 

Thank you for your reply 

Best regards 
Sankar.k

For more options, visit https://groups.google.com/d/optout.


--
shankar

Lakshman

unread,
Feb 25, 2016, 6:09:27 AM2/25/16
to material...@googlegroups.com

There is no code for the same,

However as suggested by some of our friends, same WPS can be used for 1 or 2 layer deposition.

And regarding heat treatment – it depends on the MOC, flange size, thickness, deposited weld thickness, and any more heat treatment done during manufacturing etc has to be reviewed,

And finally – convince client once again  - that it is some tolerance matter and pipe ovality issue and not the flange concern.

If the pressure ratings are of nominal, than no need of all these manipulation, you can directly weld it.

 

Thanks & Regards,

Lakshman Kumar B,

+91 9440031459.

 

From: material...@googlegroups.com [mailto:material...@googlegroups.com] On Behalf Of sankar bombay


Sent: Thursday, February 25, 2016 3:18 PM
To: material...@googlegroups.com

Reply all
Reply to author
Forward
0 new messages