impact results - UHT material welding

47 views
Skip to first unread message

Fernando L Neto

unread,
Jun 30, 2016, 1:07:42 AM6/30/16
to material...@googlegroups.com
Dear colleagues, 

I hope this email finds all you well

Project: ASME VIII- Pressure vessel - material ASME SA517 Gr B. Thickness 9,5 mm.

 I have to qualify a WPS for welding ASME SA517 - B with impact requirements at -40 C, 

Also is required PWHT, and my first results of impact test @-40C of test plate were very low. (lateral expansion less than 0,2mm and energy less than 20J)

The declared Values of certificate of consumable is 75J @ -73C  !!!

Can the presence of PWHT changes so much the values of impact test? (certificate´s value is "as welded" and my results is "after PWHT".

Any help will be very useful. 

Thanks a lot, 

Fernando Lescovar Neto (IWE)




Kannayeram Gnanapandithan

unread,
Jun 30, 2016, 4:16:10 AM6/30/16
to materials-welding
yes in Q&T steel,. before taking up for PWHT, better consult manufacturers for temperature and Time

THANKS & BEST REGARDS,
KG.PANDITHAN, IWE,  AWS-CWI, CSWIP 3.1,
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

--
http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANv%2BETZM4c_%3Dh%2BeKOosPusHUqGE_5b0DZ3aO12GyNDPph3dUbw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.

Alan Denney

unread,
Jun 30, 2016, 11:01:17 AM6/30/16
to material...@googlegroups.com

--

http://www.linkedin.com/groups/MaterialsWelding-122787?home=&gid=122787&trk=anet_ug_hm
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To post to this group, send email to material...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/CANv%2BETZM4c_%3Dh%2BeKOosPusHUqGE_5b0DZ3aO12GyNDPph3dUbw%40mail.gmail.com.
For more options, visit https://groups.google.com/d/optout.


This email has been scanned by BullGuard antivirus protection.
For more info visit www.bullguard.com

pgoswami

unread,
Jun 30, 2016, 11:41:51 AM6/30/16
to material...@googlegroups.com

Hi Fernando,

 

Welding of 517 grades is never easy. It becomes difficult when impact properties are in question. If you could share details about (MTR) the materials, welding consumable, and the failed PQR, then there could be some meaningful suggestions provided.

 

Thanks.

 

 

 

Pradip Goswami, P.Eng,IWE
Independent Welding & Metallurgical Engineering Specialist ,
Ontario,Canada.
ca.linkedin.com/pub/pradip-goswami/5/985/299

pgos...@quickclic.net

pradip....@gmail.com

 


To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/000e01d1d2ab%246c198f30%24444cad90%24%40denney1.freeserve.co.uk.
Reply all
Reply to author
Forward
0 new messages