Dear Mr. Shashi kumar,
 
I have attached the spec sheet of Alloy-20 for your reference.Usually this alloy is a fully austenitic alloy, so requires good cleanliness to ensure crack free(usually hot cracks) welds. Usually welding consumable should have low residuals ( S & P). E-320 and ER-320LR consumables are fine.
 
Usually this alloy does not require preheating, for barrier layer deposition on 4" thick flange preheating (100-150 deg C)  is recommended. If this deposition is a multi layer deposition, 2nd layer onwards in the interpass should be controlled 150 deg C max. Clearing LPI is recommended for each pass of weld deposition.
 
Due to high nickel content the wetting behavior of this alloy can be a problem, hence proper bead overlap (40-50 %) would ensure a sound defect free weld deposit.
 
Looking at the problem, the defect looks to me as improper fusion or lack of interbead fusion. If you do a light grinding ,then improper fusion would be reveled, otherwise LPI would detect it.
 
Look forward to further feedback from your end.
 
Thanks  

 

Pradip Goswami,P.Eng

Senior Engineer/Specialist(Welding-Metallurgy)

Machine Dynamics & Component Integrity Dept.

Engineering & Training Services Division

ONTARIO POWER GENERATION Inc.

PO Box-2000, RR-55(South)

Nanticoke, Ontario,N0A1L0

Tel:-(519) 587-2201, Ext 3107--in Nanticoke

         (416) 231-4111, Ext 5925--in Kipling,Toronto

Fax: (519) 587-6814

Email-prad...@opg.com.

 
 


From: pro...@cicb-chemicon.com
To: material...@googlegroups.com
Date: Mon, 23 Nov 2009 11:07:26 +0530
Subject: [MW:3712] Carpenter steel Alloy20 welding

Dear Gentlemen,

 

Is preheat of work piece required for Alloy20 overlay on P1 (100 thk Girth flange)

using ER-320LR and for welding of Alloy 20 plates.

I am Experiencing Lot of defects in welding of Alloy 20 plates SB 463 / 16 thk .

Defects are linear but are not actually slag.

What could they be???

Consumable used is E-320 and ER-320LR.

 

Will appreciate immediate response.

 

Regards,

Shashi kumar

 


Please don't print this e-mail unless you really need to.
*******************************************************************
This e-mail is confidential. It may also be legally privileged. If you are not the addressee you may not copy, forward, disclose or use any part of it. If you have received this message in error, please delete it and all copies from your system and notify the sender immediately by return e-mail. Internet communications cannot be guaranteed to be timely, secure, error or virus-free. The sender does not accept liability for any errors or omissions.
*******************************************************************
"SAVE PAPER - THINK BEFORE YOU PRINT!"

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.

20Cb-3R Stainless.pdf

Prodmlr

unread,
Nov 23, 2009, 11:33:07 PM11/23/09
to material...@googlegroups.com

Dear Mr.Pradip,

 

We are using LR type filler material .

I have read that these repairs are nothing but oxides and avoiding these is very difficult.

Is it true.

 

Regards,

Shashi Kumar