I have confusion about validity for the welder qualification.

As per ASME Sec-IX, QW-322, When welder has not welded withe process
during the period of 6 months or more his qualification for that
process shall expire unless within 6 months period prior to his
expiration of qualification.

i have doubt that if welder is doing welding for particular process
since 1 yr under my supervision, the will i need some renewal?

shall the welder expired or not within 6 months period if he is doing
welding for particular process:

Kindly justify this clause


Regards,

Ankit Khatri

Feroz Mohammed

unread,
Feb 18, 2012, 12:48:46 AM2/18/12
to material...@googlegroups.com
You may requalify him or may continue as him, also depends on customer & contractor mutual agreement.


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--
Thanks & Regards
Feroz Mohammed
Deputy Manager-QA&I
LANCO Infratech Ltd.

SENTHILKUMAR SWAMINATHAN

unread,
Feb 18, 2012, 4:07:38 AM2/18/12
to material...@googlegroups.com
You can renew it with record proof within the 6 months period where RT or UT accepted on his weld.
 
Regards,
S.SENTHILKUMAR
From: Feroz Mohammed <fero...@gmail.com>
To: material...@googlegroups.com
Sent: Saturday, 18 February 2012 6:48 AM
Subject: Re: [MW:13728] For expiration of welders for WPQ

Prasad Ghanekar

unread,
Feb 18, 2012, 4:03:23 AM2/18/12
to material...@googlegroups.com
1. You need to requalify if welder if he has not welded with the process qualified during the period of 6 month.
 
2. Continuty of welder must be demonstrated by keeping records of  weldment made by a welder with the process qualified. This is generally supported by NDE (RT) records of the satisfactorily made weldments by the welder.
 
Regards,
 
Prasad

On Fri, Feb 17, 2012 at 5:29 PM, khatri ankit <nids01...@gmail.com> wrote:

S.Sundar Rajan

unread,
Feb 18, 2012, 7:46:16 AM2/18/12
to material...@googlegroups.com
Dear Mr.Ankit,

Upon satisfactory performance of the welder you can renew his qualification for every six month without re-qualification. But if the welder has the gap of more than six month in welding or any question arises on his performance, then the welder should be requalified to demonstrate his skills and ability.
 
 
With Regards,
s.sundarrajan,
QA/QC Inspector,
Special technical services LLC, Muscat,


From: khatri ankit <nids01...@gmail.com>
To: Materials & Welding <material...@googlegroups.com>
Sent: Friday, 17 February 2012 3:59 PM
Subject: [MW:13725] For expiration of welders for WPQ
--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-welding+unsub...@googlegroups.com

kannayeram gnanapandithan

unread,
Feb 19, 2012, 8:09:53 AM2/19/12
to material...@googlegroups.com
maintain continuity record of welder for that process , that is enough
evidence that he is on the process
Pandithan
Cethar Ltd

> materials-weld...@googlegroups.com


> For more options, visit this group's bolg at
> http://materials-welding.blogspot.com/
> The views expressed/exchnaged in this group are members personel views and
> meant for educational purposes only, Users must take their own decisions
> w.r.t. applicable code/standard/contract documents.
>

> --
> To post to this group, send email to material...@googlegroups.com
> To unsubscribe from this group, send email to

> materials-weld...@googlegroups.com

Reply all
Reply to author
Forward
0 new messages