P No- 1 Material

100 views
Skip to first unread message

Rana, Jignesh

unread,
Nov 23, 2009, 8:24:08 AM11/23/09
to material...@googlegroups.com
 
Dear All,
 
I have an equipment to be installed in sour services.
 
Material – SA 516 Gr. 70 (HIC tested plates), 132 mm thickness.
 
For PWHT the soaking time is 5.30 Hrs as per project specification. Considering one cycle for future site / modification requirement, the total simulation time works out to be 11 Hrs.
 
PWHT Temperature – 620 Deg .C.
 
What would be behavior of material below LOWER TRANSFORMATION TEMPERATURE (P No. 1), against this cycle? (Tensile property, Impact property).
 
All reputed mills are denying for supply with the simulated testing condition (620 DEG C and 11 Hrs. Soaking Time).
 
Regards,
 
JIGNESH R RANA
 

Messages sent by email can be manipulated by third parties and are therefore generally not legally binding. This message contains confidential information that may be privileged or protected from disclosure. If you are not the intended recipient, please be advised that you have received this email by mistake. You are requested to notify us immediately by return email and delete this email from your system. Any use, copying, distribution or printing of information by the unintended recipient is strictly prohibited. Thank you.

Regd. Office: Uhde House, Vikhroli (West), Mumbai 400 083, India
Tel: 91-022-6796 8000, Fax: 91-022-2578 4327 Website: www.uhdeindia.com

pgos...@sympatico.ca

unread,
Nov 23, 2009, 6:54:31 PM11/23/09
to material...@googlegroups.com


Hello JIGNESH

 

I have attached the requirements of ASME Sec-VIII,DIV-1 and DIV-2 on simulation test coupons.DIV-2 is more specific for simulation heat treatment coupon than DIV-1.From my past experiences in major fabrication shops in India, I came across scenarios where the simulations test coupons had to be procured and tested by the fabricator. Mills may do it ,but at extra cost.

 

For a service as mentioned below:-

 

·         Material – SA 516 Gr. 70 (HIC tested plates), 132 mm thickness.

·         PWHT:- the soaking time is 5.30 Hrs as per project specification. Considering one cycle for future site / modification requirement, the total simulation time works out to be 11 Hrs.

·         PWHT Temperature – 620 Deg .C.

·         What would be behaviour of material below LOWER TRANSFORMATION TEMPERATURE (P No. 1), against this cycle? (Tensile property, Impact property).

 

The properties which may change significantly after 11 hrs simulation HT @  620 Deg C  would be charpy  impact and hardness test properties. Impact may significantly increase and hardness may reduce so as to stay below the project spec for sour service. Clean chemistry of the steel is very important. The following specifications might be of help to you:-

 

·         NACE –Publication 8 X 194—Materials and Fabrication Practices for New Pressure Vessels used in wet H2S service.

·         TM0284-2003-Evaluation of Pipeline and Pressure Vessel Steels-HIC

·         NACE Standard TM0103-2003- Laboratory Test Procedures for Evaluation of SOHIC Resistance of Plate Steels Used in Wet H2S Service

 

 

Thanks

 

 

 

Pradip Goswami,P.Eng

Senior Engineer/Specialist(Welding-Metallurgy)

Machine Dynamics & Component Integrity Dept.

Engineering & Training Services Division

ONTARIO POWER GENERATION Inc.

PO Box-2000, RR-55(South)

Nanticoke, Ontario,N0A1L0

Tel:-(519) 587-2201, Ext 3107--in Nanticoke

         (416) 231-4111, Ext 5925--in Kipling,Toronto

Fax: (519) 587-6814

Email-prad...@opg.com.

 

Sec VIII, DIV-1-UCS-85(h) The simulation of cooling rates for test specimens from non impact tested materials 3 in. and under in thickness is not required for heat treatments below the lower transformation temperature.

 

 

Sec VIII, DIV-2-Provisions of Sample Test Coupons

When material is subjected to heat treatment during fabrication, the test specimens required by this Division shall be obtained from sample coupons which have been heat treated in the same manner as the material, including such heat treatments as were applied by the material producer before shipment. The required tests may be performed by the material producer or the fabricator.

 

  


From: jign...@thyssenkrupp.com
To: material...@googlegroups.com
Date: Mon, 23 Nov 2009 18:54:08 +0530
Subject: [MW:3715] P No- 1 Material

 

Dear All,

 

I have an equipment to be installed in sour services.

 

Material – SA 516 Gr. 70 (HIC tested plates), 132 mm thickness.

 

For PWHT the soaking time is 5.30 Hrs as per project specification. Considering one cycle for future site / modification requirement, the total simulation time works out to be 11 Hrs.

 

PWHT Temperature – 620 Deg .C.

 

What would be behaviour of material below LOWER TRANSFORMATION TEMPERATURE (P No. 1), against this cycle? (Tensile property, Impact property).

 

All reputed mills are denying for supply with the simulated testing condition (620 DEG C and 11 Hrs. Soaking Time).

 

Regards,

 

JIGNESH R RANA

 


Messages sent by email can be manipulated by third parties and are therefore generally not legally binding. This message contains confidential information that may be privileged or protected from disclosure. If you are not the intended recipient, please be advised that you have received this email by mistake. You are requested to notify us immediately by return email and delete this email from your system. Any use, copying, distribution or printing of information by the unintended recipient is strictly prohibited. Thank you.

Regd. Office: Uhde House, Vikhroli (West), Mumbai 400 083, India
Tel: 91-022-6796 8000, Fax: 91-022-2578 4327 Website: www.uhdeindia.com


--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personnel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



THIS MESSAGE IS ONLY INTENDED FOR THE USE OF THE INTENDED RECIPIENT(S) AND MAY CONTAIN INFORMATION THAT IS PRIVILEGED, PROPRIETARY AND/OR CONFIDENTIAL. If you are not the intended recipient, you are hereby notified that any review, retransmission, dissemination, distribution, copying, conversion to hard copy or other use of this communication is strictly prohibited. If you are not the intended recipient and have received this message in error, please notify me by return e-mail and delete this message from your system. Ontario Power Generation Inc.

Chaitanya Purohit

unread,
Nov 23, 2009, 11:55:31 PM11/23/09
to material...@googlegroups.com
I am giving my opinion based on experience.

As HIC requirements are there PWHT has to be carried out at minimum 620 C to maintain the hardness within limit. On the other hand thickness of Plate is 132mm where after simulation of 11 hrs Tensile properties goes down specially in core (middle crosssection of plate). When tensile test from 1/4 T or 1/2 T taken there are possibility that UTS value goes below 485MPa.

Solutions

1)If client spec does not specify for simulation of extra cycle, ask mill to do test for reference and if pass no issues. If it fails just keep those value for reference.

2)Try to convinve Client to accept the PWHT Cycle with lower soaking time (ASME). I am not sure which design / manufacturing code is being used.

3)Check with design people if you use Gr 60 or Gr 65 instead of Gr 70, so that dropping of tensile strength can be taken care. These grades Mills can supply easily

Regards.
CK

   

2009/11/23 Rana, Jignesh <jign...@thyssenkrupp.com>

--
To post to this group, send email to material...@googlegroups.com
To unsubscribe from this group, send email to materials-weld...@googlegroups.com
For more options, visit this group's bolg at http://materials-welding.blogspot.com/
The views expressed/exchnaged in this group are members personel views and meant for educational purposes only, Users must take their own decisions w.r.t. applicable code/standard/contract documents.



--