STEEL GRADES S460NL & S500ML

146 views
Skip to first unread message

Hani Al Masry

unread,
Nov 4, 2018, 12:29:45 PM11/4/18
to material...@googlegroups.com
Dear Exerts 

what is Steel Grades S460NL & S500ML Are this is CS or it is alloy steels like HARDOX , WELDOX and now they call it Domex?

what is it is specification ? standards? recommended usage and applications?

Regards,
H.A

rajesh kaswala

unread,
Nov 6, 2018, 1:53:05 AM11/6/18
to material...@googlegroups.com
  S460NL acc. to DIN EN 10025-3 Mat.no. 1.8903 S460NL is a weldable, normalised steel for steel constructions, with high yield strength combined with high toughness to save weight in use.
 Delivery with certificate 3.1 to DIN EN 10204. 
Chemical composition (heat analysis %) Grade C max. Si max. Mn P max. S max. Al min. Cr max. Mo max. Cu max. Ni max. V max. N max. Nb Ti S460NL 0,20 0,60 1,00- 1,70 0,025 0,020 0,020 0,30 0,10 0,55 0,80 0,20 0,025 0,05 % 0,05% 
Mechanical properties in delivery condition Tensile testing on transverse specimens at room temperature Grade R m (MPa) ReH (MPa) A5 (% min.) 
Thickness mm  100 > 100  200  16 > 16  40  40  63 > 63  80 > 80  100 > 100  150 S460NL 550 - 720 530 - 700 460 440 430 410 400 380 17 
impact values (KV) carbon equivalent values (CEV) transverse 27 Joule -50°C  63 mm 0,53 longitudinal 16 Joule -50°C  63  100 mm 0,54 

  regard
rajesh

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
Visit this group at https://groups.google.com/group/materials-welding.
For more options, visit https://groups.google.com/d/optout.

Hani Al Masry

unread,
Nov 7, 2018, 7:33:10 AM11/7/18
to material...@googlegroups.com
HOW ABOUT   S500ML 
What is M and L OR NL OR ML
Can you send me the copy of standards of each one?
also EN 10025-4:2004  and DIN EN 10025-3 which you refer to?

Regards,
H.A
 

Kannayeram Gnanapandithan

unread,
Nov 7, 2018, 11:56:47 PM11/7/18
to material...@googlegroups.com
M---Thermomechanically treated. Generally there are 3 impact requirements in joules. J, K, L. 27joules for J. 40joules for K & 60joules for L at tested temp. For more understanding pl ref EN 10020

Hani Al Masry

unread,
Nov 8, 2018, 9:34:06 PM11/8/18
to material...@googlegroups.com
N?