parent mental is 25crmo4 to 25crmo4. Is 80S-B2 filler material is suitable or anything else one plz suggest

125 views
Skip to first unread message

Mehul Patel

unread,
Sep 15, 2024, 6:04:55 AM9/15/24
to Materials & Welding
Dear Experts'


Plz suggest me filler metal for 25crmo4 & explain 80S-B2. 

Vishwas Keskar

unread,
Sep 15, 2024, 8:16:42 AM9/15/24
to material...@googlegroups.com
Pl send details of mechanical and chemical properties of the base metal - 25 CrMo4
Pl detail out service conditions of components being fabricated 
Any specific application?
Thanks 
Vishwas - IWE 

9823472273
Sent from my iPhone

On 15 Sep 2024, at 3:34 PM, Mehul Patel <vmgm...@gmail.com> wrote:

Dear Experts'


Plz suggest me filler metal for 25crmo4 & explain 80S-B2. 

--
https://materials-welding.blogspot.com/
https://www.linkedin.com/groups/122787
---
You received this message because you are subscribed to the Google Groups "Materials & Welding" group.
To unsubscribe from this group and stop receiving emails from it, send an email to materials-weld...@googlegroups.com.
To view this discussion on the web visit https://groups.google.com/d/msgid/materials-welding/168bfb14-9d86-4c3a-84d5-45ad0c8f4224n%40googlegroups.com.

Mehul Patel

unread,
Sep 16, 2024, 5:31:40 AM9/16/24
to Materials & Welding
1. General property which is found on 25Crmo4 material.
2. General application 

Kannayeram Gnanapandithan

unread,
Sep 17, 2024, 12:03:40 PM9/17/24
to material...@googlegroups.com
25CrMo4 is equivalent 0.25%C, 1%Cr, 0.25% Mo which almost matches ur rod selection 80S-B2
THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015, ISO 3834, EN 15085, 
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349


On Sun, Sep 15, 2024 at 3:34 PM Mehul Patel <vmgm...@gmail.com> wrote:
Dear Experts'


Plz suggest me filler metal for 25crmo4 & explain 80S-B2. 

--

vignesh musical

unread,
Sep 17, 2024, 12:31:31 PM9/17/24
to material...@googlegroups.com
Dear 

1. TIG/MIG Welding:ER80S-B2: A filler wire designed for welding Cr-Mo steels. It has good creep resistance and is suitable for high-temperature applications.ER90S-B3: This wire provides higher strength and creep resistance than ER80S-B2 and is appropriate for critical applications where higher tensile strength is needed.

Kannayeram Gnanapandithan

unread,
Sep 17, 2024, 10:47:19 PM9/17/24
to material...@googlegroups.com
90S-B3 is overmatched. B3 weld chemistry is 2.25Cr + 1Mo
Not necessary. 80S-B2 is more than enough.

THANKS & BEST REGARDS,
KG.PANDITHAN, BE, IWE,  CSWIP 3.1,
ISO 9712 Level 2 in VT,
ASNT-Level II in PT,MT,RT & UT,
LA ISO 9001-2015, ISO 3834, EN 15085, 
International Welding Engineer. 
CONSULTANT-WELDING & QUALITY
Mobile no: +919940739349

sridhar cn

unread,
Sep 19, 2024, 11:45:05 AM9/19/24
to material...@googlegroups.com
Mr. Mehul Patel,
For welding 25CrMo4 steels, a 175 to 250-degree C preheat is suggested to avoid  
hot cracks, martensite forming, and residual stress concentration. Avoid rapid cooling  
to control increased hardness and brittleness.
E/ER 80S B2 contains around  0.08% C, 1.30% Cr, 0.55% Mo, and UTS & YS are 590 
& 490 MPa, and compatible with base metal.
Sridhar.


On Sun, 15 Sept 2024 at 15:34, Mehul Patel <vmgm...@gmail.com> wrote:
Dear Experts'


Plz suggest me filler metal for 25crmo4 & explain 80S-B2. 

--
Reply all