I too had similar problems except with white, blue, aqua and I too have refused to use it in any of my printers.
I noticed debris in the filament that was the eventual cause of the blockage and failure, also the white was of such varying quality in terms of melting point it was weird. It would only flow smoothly from about 182-187, lower than 182 and it wouldn't extrude because it was too thick, 188 + it actually flowed like water out of the nozzle without even running the extruder. Also it actually bonded to the blue tape and leached all the color out of it.
Now other people have gotten good batches, and I bet they'll keep using it until they get a bad batch, but I agree that it's not worth a clogged/ruined hot end for the money your saving.
Personally I buy my ABS from 3dPrinterStuff, my PLA from Ultimachine and have had absolutely zero problems from either vendor.